  4. Falling Insulation Resistance Is Not Always Water Ingress - Three Conditions for Electrochemical Migration, Two Look-Alike Paths, and the Right Order of Fixes

Falling Insulation Resistance Is Not Always Water Ingress - Three Conditions for Electrochemical Migration, Two Look-Alike Paths, and the Right Order of Fixes

Key takeaways

Only three paths connect two conductors - a water film, ionic residue, or actual metal migration. Drying fixes the first, washing fixes the second, and only what survives both is migration. Migration requires ionic contamination, a water film and a bias voltage at the same time; remove one and it cannot occur. So the first question is whether the test was powered, not how much water got in.

A failed insulation resistance reading is almost always blamed on water ingress. But only three paths connect two conductors: a film of water on the surface, ionic residue left on the board, and metal that has actually grown across. The first two are reversible - dry the board or wash it and the reading returns. The third is not; once a dendrite bridges the gap, washing changes nothing. Only that third path is electrochemical migration, and it needs three things at once: ionic contamination, a water film and a bias voltage. Remove any one and it cannot happen. The useful first question is therefore not how much water got in, but whether the test was powered and whether the board was clean.

1. Three paths, and how to tell which one you have

What separates the three paths is not how they look but whether they can be reversed. What reverses is physical adsorption; what does not is a chemical or metallurgical process. The remedies are entirely different.

Conductive pathConducting mediumAfter drying / after washingWhere the evidence sits
------------
Surface water filmCondensation, adsorbed waterRecovers / no wash neededReading tracks humidity and returns when the environment changes
Ionic residueFlux, cleaning agent, fingerprints, plating saltsMostly does not recover / recoversVisible residue, elevated ionic contamination
Metal migrationDendrite, conductive channel inside the laminateDoes not recover / does not recoverDiscolouration, dendrites, channel or carbonised laminate in cross-section

Read the table backwards. Check whether the reading recovers after drying; if it does, stop there. If it does not, wash the board and measure again - recovery after washing means contamination, and only a reading that survives both steps is migration. Jumping straight to microscopy usually produces a folder of images that show a phenomenon without explaining it.

All three paths can coexist on one board. A surface water film makes the salts on the board dissociate more readily, so migration accelerates as well. A low reading taken with condensation present is evidence of "wet right now", not evidence of "already migrated".

2. Migration requires all three conditions

ConditionIf it is missingWhich test or process variable controls it
---------
Ionic contamination (flux, cleaning agent, plating salts, fingerprints)Even a thick water film carries no charge carriers; the drop is a humidity effectCleaning process and cleanliness verification
Water film (condensation, adsorbed water, capillary pooling)Ions cannot travel and stay where they areTemperature-humidity profile, recovery conditions, drainage design
Bias voltage (DC field between two conductors)No driving force, so metal neither dissolves nor deposits directionallyPowered or unpowered, bias source, polarity, applied nodes

These three multiply rather than add. Remove one and nothing migrates - which is why the same board can receive opposite verdicts from two laboratories. One ran damp heat unpowered, the other ran it under bias. Both called it 85/85; they tested two different things.

Direction is set by the field, so polarity is not a detail. A single fixed polarity only transports metal on one side; run long enough in one direction and the more sensitive structure on the other side is never exposed. Some corporate specifications require reverse or alternating bias for exactly this reason. Whether it applies, and how it is scheduled, follows the customer specification and the technical agreement.

3. Damp heat without bias never reaches this chain

Environmental test standards generally specify the temperature-humidity profile and the duration. Whether bias is applied, where it comes from, and whether the working voltage or a separate test voltage is used are normally set by the corporate specification or the technical agreement. Leave that column blank and the laboratory applies its default - samples unpowered - and the chain is never exercised.

ItemTwo common practicesIf it is left unspecified
---------
Bias appliedUnpowered / powered with biasThe report says "damp heat passed" when migration was never tested
Bias sourceWorking voltage / separate test voltageResults from two laboratories are not comparable
PolarityFixed / reverse / alternatingA structure sensitive on one side only is missed
Monitoring and recoveryIn-chamber monitoring / measurement after removalThe day a short occurred cannot be established

One more point is easily missed: how samples are arranged inside the chamber. Stacking, standing against a wall, or coiling a harness on top of a sample all change local condensation, so differences within a batch may come from placement rather than design. With bias applied, feed-through wiring has to be handled as well - the seal and the insulating support at the chamber port are leakage paths in their own right. When a reading is low, suspect them before suspecting the board.

Recovery conditions must also be written down. A sample straight out of the chamber carries condensation, so its insulation resistance will read low; leave it in a clean environment for a while and the number climbs noticeably. Both readings are "true" and neither is comparable to the other. The outline should state the recovery duration, the recovery environment, and whether measurement happens before or after recovery.

4. Reading the number: not a matter of waiting longer or reading sooner

Once a DC voltage is applied, the current through the sample has three parts: charging current of the geometric capacitance, dielectric absorption current, and true leakage current. The first two decay with time, so the reading climbs and only settles at the leakage value. Recording the number as soon as the voltage is applied captures an intermediate state of the charging process and reads lower than the true value. That is why specifications require the reading to be taken at stability.

Four factors decide whether a reading means anything:

  • Test voltage: chosen per the standard or the agreement, not turned up on a hunch. A higher voltage can activate a defect that was not yet connected, and the board can no longer be treated as undamaged afterwards.
  • Stability criterion: state when the reading counts as stable. If two runs of the same project use different criteria, the data cannot be joined.
  • Nodes and circuit: state which two conductors are measured and whether the housing, shield or connector shell is included. Results from different circuits do not substitute for one another.
  • Temperature and humidity at measurement: the same board can differ by an order of magnitude between humidity levels, so the record must carry the ambient conditions.

The acceptance value usually comes from the corporate specification or the technical agreement; environmental test standards provide the profile and the method, not necessarily a number. A trend is more convincing than an absolute value: same node, same conditions, before and after the test. A drop of an order of magnitude deserves investigation even when it stays within the limit.

5. Order of fixes: wash first, then the design, then coating

There are four steps, and getting the order wrong wastes money or makes things worse.

  1. Confirm it is contamination. Ionic residue can be washed off. Cleanliness verification - ionic contamination measurement and board residue inspection - costs far less than coating and is easier to falsify.
  2. Then look at the design. Pooling cavities, capillary gaps, dead zones at connector roots. Changing drainage paths and creepage distances takes longer, but it is the actual cure.
  3. Only then coat. Conformal coating blocks the water film, not the ions. Coating an unclean board seals the electrolyte underneath, moving migration from the surface to beneath the film where it is harder to find.
  4. Close with spacing and shielding. Layout changes have the longest lead time and are usually reserved for residual cases after the first three steps.

Incomplete coverage is often worse than no coating. Edges, connector roots, vias and the perimeter of large pads that are left uncovered become local anodes, and corrosion concentrates there - it looks as if the coating did nothing, when in fact it concentrated the problem.

A few plain words

The hard part of this chain is not the acceptance criterion but identifying which path you are on. Dry, wash, measure - three steps settle most disputes, and only what survives them needs cross-sectioning and composition analysis.

  • Check recovery after drying first, then recovery after washing;
  • Damp heat without bias tests moisture absorption, not migration;
  • Bias source, polarity, monitoring and recovery belong in the outline, or the report has nothing to compare against;
  • Coating is not a substitute for cleaning; it is the line of defence after cleaning.

When TMC LAB takes on damp heat or salt spray work under bias, the bias source, applied nodes, polarity, in-chamber monitoring items and recovery conditions are written into the test outline and confirmed before samples enter the chamber. The test voltage and stability criterion for insulation resistance are fixed at the same time, so two readings from the same project can be compared. Acceptance values follow the customer specification and the technical agreement; no values are preset at the outline stage.

To sort out the profile itself first - steady-state damp heat and cyclic damp heat are not the same test - see the comparison of the two damp heat profiles. How salt spray duration is set is covered in the salt spray article, and chemical agents with cleaning-agent residue belong to another line, with conditions in chemical loads. The relationship between ingress protection and condensation is set out in IP6K9K versus IP69K.

For clause-level breakdowns, see the GB/T 28046 and ISO 16750 standard pages. The two service scopes are damp heat testing and salt spray and corrosion, with ingress protection under IP ratings.

Scheduling is arranged per project; you can state your expected delivery date when submitting samples, and we will confirm a feasible plan against the current schedule and report progress at each milestone.

Related Q&A

Related questions

Frequently asked questions on the same topic. The first paragraph of each answer is the conclusion.

When insulation resistance fails, how do I tell water ingress from electrochemical migration?
Work backwards through two steps - dry, then wash. First dry the sample thoroughly in a clean environment and measure again; a clear recovery means a surface water film, a reversible change caused by condensation or high humidity. If it does not recover, clean the board surface and retest; recovery after washing points to ionic contamination such as flux or cleaning-agent residue. Only if the reading stays low after washing, with discolouration, dendrites, or a conductive channel visible in cross-section, is it metal migration. Skipping the first two steps and going straight to microscopy usually produces images that show a phenomenon but cannot explain its cause.
Can a damp heat test without bias detect electrochemical migration?
Essentially no. Migration requires ionic contamination, a water film and a DC electric field at the same time; without the field there is no driving force, and metal neither dissolves nor deposits directionally. A damp heat test without bias examines moisture absorption, material degradation and sealing integrity - the sample is unpowered in the chamber, so the migration chain is never exercised. Two tests both called damp heat therefore cannot substitute for each other. Whether bias is applied, where it comes from, its polarity, the nodes it reaches and how the sample is monitored all belong in the technical agreement.
If a board is at risk of electrochemical migration, can I just apply conformal coating?
Not recommended. Conformal coating blocks the water film, not the ions. Coating a board that still carries flux or cleaning-agent residue seals the electrolyte underneath the coating, moving migration from the surface to beneath the film and making failures harder to locate. The correct order is to verify cleanliness first, confirm ionic residue has fallen to an acceptable level, then review the design for pooling cavities and capillary gaps, and only then coat. Incomplete coverage is often worse than no coating at all - edges, connector roots and uncovered via areas become local anodes, and corrosion concentrates there.

These answers share the same data source as the FAQ page.

Have a testing requirement? Send us your product details

Tell us the product model and test requirements. Our engineers will map out the test plan, the applicable standards and the item combination, and provide a quotation reference. The more specific the request, the sharper the answer.

  • Free scoping of the test plan and standards
  • Pre-scan testing during R&D to cut rework cost
  • On-site visits and witnessed testing supported
  • Scheduling per project, with progress updates at each milestone

Received — we will contact you shortly and follow up with a test plan and quotation.

By submitting you agree to be contacted by phone or email. Scheduling follows the project’s actual availability and is subject to mutual confirmation.

13510907826
Call