Key takeaways
A failed part begins to change the moment it is removed, and what changes is the evidence rather than the fault. Fracture topography is lost in packaging, through bubble wrap pressed directly on the break, labels on the fracture face, or bare fingers. Electrical and surface state is lost in transit and storage, through plain bags, humidity and condensation. Comparability is lost by mixing, when the failed part and the batch reference share one bag and the labels disappear. Packaging has to block four things: mechanical contact, static, moisture and loss of identity. Fracture faces must not be washed, taped or touched. Disassembly has three levels, from module to board to device or section, and each step is less reversible. On arrival, photograph the package before opening, count the contents, let cold parts reach room temperature before opening, then register the failed part and the reference parts under separate numbers. Damage that appears in batches with a consistent direction usually comes from transit; single damage along a stress path is the original failure.
A failed part starts changing the moment it is removed from the vehicle. What changes is not whether it is broken, but how much evidence is left. From the bench to the packaging, from the packaging to the courier, from the courier to the storage shelf, each stage destroys a different kind of evidence: the original topography of the fracture, the electrical and surface state of the part, and its comparability with the rest of the batch. Once those three are gone, the cleanest cross-section in the world still only supports the sentence "damage was observed", never "damage was caused by".
A typical purchase order says: one failed part, please determine the cause. That single line omits three things: how the part was removed, how it was packed, and what state it was in on arrival. None of the three lives inside the part, yet all three can rewrite the conclusion. The laboratory receives an arrival condition, not a failure scene, and treating the two as the same thing is where most disputes actually begin.
Handling of a failed part is the input stage of failure analysis. Get the input wrong and every later step is judging an object that has already changed.
1. Evidence does not start disappearing on the cross-sectioning table
Most teams concentrate on sectioning and interpretation, because that stage is visible, instrumented and photographed. The real loss happens earlier and much more quietly.
| Evidence lost | Where it is usually lost | What happens afterwards |
|---|---|---|
| --- | --- | --- |
| Original fracture topography | Part left loose on a bench, bubble wrap pressed on the break, label stuck on the fracture face | Compaction marks and parallel scratches overwrite the basis for reading dimples, cleavage or intergranular separation |
| Electrical and surface state | Bare-hand handling, plain plastic bags, storage in humid air, a cold part opened immediately | Leakage paths, oxide films and dendrites are added or wiped away, and electrical re-test no longer reproduces the in-vehicle behaviour |
| Comparability with the batch | Failed and good parts in one bag, lost labels, loose accessories | Batch-wide versus single-case cannot be separated, the reference is gone and the conclusion cannot be extended |
Failure inside the chamber, in the first ten minutes, is covered separately in what to do when a sample fails during test. That article stays at the chamber. This one covers the next stretch: the part has left the site and is on the road, in a courier box, or on a shelf waiting to be opened.
2. Packaging blocks change, not the part
"Pack it better" has no execution value. Packaging has to block four specific changes, each with its own materials and method.
| What must be blocked | Common practice | Consequence of getting it wrong |
|---|---|---|
| --- | --- | --- |
| Mechanical contact | Part located inside a rigid box, fracture side left free, dividers between parts | The fracture is compacted or polished, and the surface becomes a photograph that has been wiped |
| Static | Metallised shielding bag, pins shorted before bagging | New breakdown holes appear inside the device and sit in the same report as the original failure |
| Moisture | Desiccant, humidity indicator, heat-sealed foil bag | Condensation and oxidation can occur within days, and corrosion products end up where the test history says they cannot be |
| Loss of identity | Part marking, orientation marks, accessory list, reference parts bagged separately | Reference parts can no longer be matched to the failed part, and batch judgement loses its basis |
The fracture face is the area most often destroyed by good intentions. Three actions must be prohibited: washing, taping and touching. Washing carries away attached particles and soluble contamination, and those particles are frequently the clue to the initiation site. Tape or a label pulled off takes the top layer of the fracture with it. Finger contact leaves an oil film only molecules thick, yet energy-dispersive analysis reads carbon and oxygen first and suppresses the substrate signal.
The same rule applies at the sectioning stage: before a fracture is observed, nothing should have touched it. That discipline matters more than the grade of the packaging material.
3. Disassembly and storage come in a fixed order
Disassembly is irreversible. Every level removed takes away part of the previous level's evidence, so sequence matters more than technique: record, photograph, de-energise, disassemble; then separate, label, and only then box.
| Level of disassembly | When it is the right choice | What it costs |
|---|---|---|
| --- | --- | --- |
| Module assembly only | Electrical failures, intermittent faults, where mounting position and harness routing are themselves variables | Going further loses the installed state, and many intermittent faults appear only in that attitude |
| Down to board level | Solder joints, connectors, plating and conformal coating need to be seen | Fastener marks, indentations and fingerprints on the board are destroyed by a second touch |
| Down to device or section | Only material and fracture work, with no further electrical re-test needed | Irreversible; the electrical evidence is gone in one step and coming back means repeating the test |
Who did the disassembly belongs in the record too. Customer site, service depot and laboratory use different tools, different force and different environments, so each leaves different traces. Whether a particular scratch came from removal or existed at the moment of failure can only be answered by the disassembly record.
That record does not need to be long. Five items are enough: who, when, with what tool, to which level, and whether any new damage was noticed at each step. Its value appears only once a dispute exists, and by then it can no longer be reconstructed.
4. Damage added in transit, and how to tell it from the original failure
Transit damage is not something careful handling eliminates; it is systematic and has stable signatures. Separating it from the original failure relies on distribution patterns, not on a single observation.
| Added damage | Signature | How to separate it from the original failure |
|---|---|---|
| --- | --- | --- |
| Deformed terminals and pins | Bending direction consistent across parts, concentrated at protruding features | An original failure usually appears at one location and follows the load path; batch-wide and same-direction points to crushing |
| Contaminated or polished fracture | Parallel scratches, embedded foreign matter, rounded edges | An original fracture has initiation, propagation and final-overload zones; a polished one is a single plane |
| Electrostatic breakdown | Fresh melt holes, random location, no stress history around them | Unrelated to the working load path, no fatigue striations nearby, not at a thermal or electrical concentration |
| Moisture corrosion | Products concentrated at contact faces and gaps, pale and friable | Inconsistent with the test history: condensation-type corrosion appears where the part never saw that temperature and humidity |
One rule of thumb travels well: batch-wide, same-direction damage concentrated at protruding features points to transit; single-site damage along a stress path that matches the test profile is the original failure.
When both are present, report them separately. Counting transit damage as the cause sends corrective action in the wrong direction. Counting the original failure as transit damage lets the real problem through. Both mistakes are common in disputes, and both are avoidable with a packaging record.
Static is the one most often missed, because it frequently leaves no visible trace. A related diagnostic path is set out in reset on ESD contact, fine once released; where internal breakdown has to be confirmed without opening the part, X-ray inspection can narrow the area first.
5. Five things to do on arrival
This stage is the one most often skipped, because the part is already in hand. That half hour decides whether the later records have any reference value at all.
| Action | What to record | Why it cannot be skipped |
|---|---|---|
| --- | --- | --- |
| Photograph the packaging before opening | Dents and tears, seal condition, humidity indicator colour | In a dispute it is the only proof that the condition predates arrival |
| Weigh and count | Number of parts, accessories, packaging list | A missing or extra item changes the conclusion, and a loose accessory is often the decisive one |
| Let cold parts reach room temperature | Arrival temperature, settling conditions | A cold part condenses moisture immediately, and the condensation itself creates fresh corrosion marks |
| Photograph each layer from outside in | Outer packaging, inner packaging, part, accessories, fracture orientation | Packaging state can be reconstructed, and only then can what happened on the road be discussed |
| Register under separate numbers | Failed, batch reference and retained samples kept apart | The reference part is the basis for batch judgement, and one mixed bag destroys it permanently |
At TMC LAB, failed parts are registered in their arrival condition before an analysis route is chosen: where electrical evidence can be preserved, non-destructive inspection comes first, and where sectioning is required, a second part is retained in its original state. The sequence is not procedural neatness; electrical and fracture evidence cannot both be preserved through the same disassembly.
Storage has its own rules: a dry cabinet or low-humidity cabinet, away from light, away from reagents and cleaning agents, not sharing a cabinet with magnetic parts. A few days look like nothing, while the oxide film grows, flux residue absorbs moisture and plating keeps changing. The later the analysis is scheduled, the more this matters.
6. Five fields that must be filled in on the purchase order
| Field | What to write | What happens when it is blank |
|---|---|---|
| --- | --- | --- |
| Part count and identity | How many failed, reference and retained parts, and the numbering rule | Batch judgement becomes impossible; the allocation logic is described in sample quantity is not the laboratory's call |
| State at the time of failure | Powered or not, what load, which stress segment | The failure mechanism cannot be oriented and environmental conditions cannot be aligned; use the load categories in GB/T 28046 and ISO 16750 as the reference |
| Known disassembly history | Who removed it, to which level, any new traces | It becomes impossible to tell which evidence is already compromised, and transit marks get read as in-service marks |
| Packaging and transport | Static protection level, moisture protection, how the fracture was fixed, how many legs and days | Arrival condition cannot be reconstructed, nor whether condensation happened on the way |
| Expected analysis level | Non-destructive first or sectioning allowed, whether electrical re-test must stay possible | Sample allocation cannot be decided, and sectioning first can leave a need for electrical data that no longer exists |
The packaging and transport field is usually blank. When it is blank the laboratory can only apply a default, and the default is often wrong for the part in question: a casting with a fracture and a connector with gold contacts need opposite fixing methods.
7. A few honest words
A fracture is not renewable. Another part can be requested and another batch can be sampled, but once a fracture face is polished it never comes back. Whatever extra budget goes into packaging should go into keeping that face away from every material.
A reference part is a baseline, not a spare. A single failed part supports the statement "this one broke"; add unfailed parts from the same batch and it becomes "this is where the batch deviates". That saves more money than any packaging material.
Write transit damage into the report instead of hiding it. Hiding it swaps the object of analysis. The conclusion looks clean while the corrective action goes the wrong way. Reporting it separately is a mark of competence, not of carelessness.
A packaging record is the only thing that can speak for you in a dispute. An unboxing video, a humidity indicator and a weighing slip take under ten minutes together and decide whether a report still stands six months later.
Where the part came off a vehicle, the gap between installed and tested state is a variable in itself, and the four gaps in the test passed but the vehicle still failed are worth checking against. Judgement of the material itself belongs to materials and structure testing and is a different task from reading a fracture.
Scheduling is arranged per project; you can state your expected delivery date when submitting samples, and we will confirm a feasible plan against the current schedule and report progress at each milestone.