Skip to main content
  1. Home
  2. Technical Blog
  3. Failure Analysis
  4. The Failed Part That Arrives at the Lab Is No Longer the Part That Failed: Packaging, Transit and Storage Each Destroy a Different Kind of Evidence

The Failed Part That Arrives at the Lab Is No Longer the Part That Failed: Packaging, Transit and Storage Each Destroy a Different Kind of Evidence

Key takeaways

A failed part begins to change the moment it is removed, and what changes is the evidence rather than the fault. Fracture topography is lost in packaging, through bubble wrap pressed directly on the break, labels on the fracture face, or bare fingers. Electrical and surface state is lost in transit and storage, through plain bags, humidity and condensation. Comparability is lost by mixing, when the failed part and the batch reference share one bag and the labels disappear. Packaging has to block four things: mechanical contact, static, moisture and loss of identity. Fracture faces must not be washed, taped or touched. Disassembly has three levels, from module to board to device or section, and each step is less reversible. On arrival, photograph the package before opening, count the contents, let cold parts reach room temperature before opening, then register the failed part and the reference parts under separate numbers. Damage that appears in batches with a consistent direction usually comes from transit; single damage along a stress path is the original failure.

A failed part starts changing the moment it is removed from the vehicle. What changes is not whether it is broken, but how much evidence is left. From the bench to the packaging, from the packaging to the courier, from the courier to the storage shelf, each stage destroys a different kind of evidence: the original topography of the fracture, the electrical and surface state of the part, and its comparability with the rest of the batch. Once those three are gone, the cleanest cross-section in the world still only supports the sentence "damage was observed", never "damage was caused by".

A typical purchase order says: one failed part, please determine the cause. That single line omits three things: how the part was removed, how it was packed, and what state it was in on arrival. None of the three lives inside the part, yet all three can rewrite the conclusion. The laboratory receives an arrival condition, not a failure scene, and treating the two as the same thing is where most disputes actually begin.

Handling of a failed part is the input stage of failure analysis. Get the input wrong and every later step is judging an object that has already changed.

1. Evidence does not start disappearing on the cross-sectioning table

Most teams concentrate on sectioning and interpretation, because that stage is visible, instrumented and photographed. The real loss happens earlier and much more quietly.

Evidence lostWhere it is usually lostWhat happens afterwards
---------
Original fracture topographyPart left loose on a bench, bubble wrap pressed on the break, label stuck on the fracture faceCompaction marks and parallel scratches overwrite the basis for reading dimples, cleavage or intergranular separation
Electrical and surface stateBare-hand handling, plain plastic bags, storage in humid air, a cold part opened immediatelyLeakage paths, oxide films and dendrites are added or wiped away, and electrical re-test no longer reproduces the in-vehicle behaviour
Comparability with the batchFailed and good parts in one bag, lost labels, loose accessoriesBatch-wide versus single-case cannot be separated, the reference is gone and the conclusion cannot be extended

Failure inside the chamber, in the first ten minutes, is covered separately in what to do when a sample fails during test. That article stays at the chamber. This one covers the next stretch: the part has left the site and is on the road, in a courier box, or on a shelf waiting to be opened.

2. Packaging blocks change, not the part

"Pack it better" has no execution value. Packaging has to block four specific changes, each with its own materials and method.

What must be blockedCommon practiceConsequence of getting it wrong
---------
Mechanical contactPart located inside a rigid box, fracture side left free, dividers between partsThe fracture is compacted or polished, and the surface becomes a photograph that has been wiped
StaticMetallised shielding bag, pins shorted before baggingNew breakdown holes appear inside the device and sit in the same report as the original failure
MoistureDesiccant, humidity indicator, heat-sealed foil bagCondensation and oxidation can occur within days, and corrosion products end up where the test history says they cannot be
Loss of identityPart marking, orientation marks, accessory list, reference parts bagged separatelyReference parts can no longer be matched to the failed part, and batch judgement loses its basis

The fracture face is the area most often destroyed by good intentions. Three actions must be prohibited: washing, taping and touching. Washing carries away attached particles and soluble contamination, and those particles are frequently the clue to the initiation site. Tape or a label pulled off takes the top layer of the fracture with it. Finger contact leaves an oil film only molecules thick, yet energy-dispersive analysis reads carbon and oxygen first and suppresses the substrate signal.

The same rule applies at the sectioning stage: before a fracture is observed, nothing should have touched it. That discipline matters more than the grade of the packaging material.

3. Disassembly and storage come in a fixed order

Disassembly is irreversible. Every level removed takes away part of the previous level's evidence, so sequence matters more than technique: record, photograph, de-energise, disassemble; then separate, label, and only then box.

Level of disassemblyWhen it is the right choiceWhat it costs
---------
Module assembly onlyElectrical failures, intermittent faults, where mounting position and harness routing are themselves variablesGoing further loses the installed state, and many intermittent faults appear only in that attitude
Down to board levelSolder joints, connectors, plating and conformal coating need to be seenFastener marks, indentations and fingerprints on the board are destroyed by a second touch
Down to device or sectionOnly material and fracture work, with no further electrical re-test neededIrreversible; the electrical evidence is gone in one step and coming back means repeating the test

Who did the disassembly belongs in the record too. Customer site, service depot and laboratory use different tools, different force and different environments, so each leaves different traces. Whether a particular scratch came from removal or existed at the moment of failure can only be answered by the disassembly record.

That record does not need to be long. Five items are enough: who, when, with what tool, to which level, and whether any new damage was noticed at each step. Its value appears only once a dispute exists, and by then it can no longer be reconstructed.

4. Damage added in transit, and how to tell it from the original failure

Transit damage is not something careful handling eliminates; it is systematic and has stable signatures. Separating it from the original failure relies on distribution patterns, not on a single observation.

Added damageSignatureHow to separate it from the original failure
---------
Deformed terminals and pinsBending direction consistent across parts, concentrated at protruding featuresAn original failure usually appears at one location and follows the load path; batch-wide and same-direction points to crushing
Contaminated or polished fractureParallel scratches, embedded foreign matter, rounded edgesAn original fracture has initiation, propagation and final-overload zones; a polished one is a single plane
Electrostatic breakdownFresh melt holes, random location, no stress history around themUnrelated to the working load path, no fatigue striations nearby, not at a thermal or electrical concentration
Moisture corrosionProducts concentrated at contact faces and gaps, pale and friableInconsistent with the test history: condensation-type corrosion appears where the part never saw that temperature and humidity

One rule of thumb travels well: batch-wide, same-direction damage concentrated at protruding features points to transit; single-site damage along a stress path that matches the test profile is the original failure.

When both are present, report them separately. Counting transit damage as the cause sends corrective action in the wrong direction. Counting the original failure as transit damage lets the real problem through. Both mistakes are common in disputes, and both are avoidable with a packaging record.

Static is the one most often missed, because it frequently leaves no visible trace. A related diagnostic path is set out in reset on ESD contact, fine once released; where internal breakdown has to be confirmed without opening the part, X-ray inspection can narrow the area first.

5. Five things to do on arrival

This stage is the one most often skipped, because the part is already in hand. That half hour decides whether the later records have any reference value at all.

ActionWhat to recordWhy it cannot be skipped
---------
Photograph the packaging before openingDents and tears, seal condition, humidity indicator colourIn a dispute it is the only proof that the condition predates arrival
Weigh and countNumber of parts, accessories, packaging listA missing or extra item changes the conclusion, and a loose accessory is often the decisive one
Let cold parts reach room temperatureArrival temperature, settling conditionsA cold part condenses moisture immediately, and the condensation itself creates fresh corrosion marks
Photograph each layer from outside inOuter packaging, inner packaging, part, accessories, fracture orientationPackaging state can be reconstructed, and only then can what happened on the road be discussed
Register under separate numbersFailed, batch reference and retained samples kept apartThe reference part is the basis for batch judgement, and one mixed bag destroys it permanently

At TMC LAB, failed parts are registered in their arrival condition before an analysis route is chosen: where electrical evidence can be preserved, non-destructive inspection comes first, and where sectioning is required, a second part is retained in its original state. The sequence is not procedural neatness; electrical and fracture evidence cannot both be preserved through the same disassembly.

Storage has its own rules: a dry cabinet or low-humidity cabinet, away from light, away from reagents and cleaning agents, not sharing a cabinet with magnetic parts. A few days look like nothing, while the oxide film grows, flux residue absorbs moisture and plating keeps changing. The later the analysis is scheduled, the more this matters.

6. Five fields that must be filled in on the purchase order

FieldWhat to writeWhat happens when it is blank
---------
Part count and identityHow many failed, reference and retained parts, and the numbering ruleBatch judgement becomes impossible; the allocation logic is described in sample quantity is not the laboratory's call
State at the time of failurePowered or not, what load, which stress segmentThe failure mechanism cannot be oriented and environmental conditions cannot be aligned; use the load categories in GB/T 28046 and ISO 16750 as the reference
Known disassembly historyWho removed it, to which level, any new tracesIt becomes impossible to tell which evidence is already compromised, and transit marks get read as in-service marks
Packaging and transportStatic protection level, moisture protection, how the fracture was fixed, how many legs and daysArrival condition cannot be reconstructed, nor whether condensation happened on the way
Expected analysis levelNon-destructive first or sectioning allowed, whether electrical re-test must stay possibleSample allocation cannot be decided, and sectioning first can leave a need for electrical data that no longer exists

The packaging and transport field is usually blank. When it is blank the laboratory can only apply a default, and the default is often wrong for the part in question: a casting with a fracture and a connector with gold contacts need opposite fixing methods.

7. A few honest words

A fracture is not renewable. Another part can be requested and another batch can be sampled, but once a fracture face is polished it never comes back. Whatever extra budget goes into packaging should go into keeping that face away from every material.

A reference part is a baseline, not a spare. A single failed part supports the statement "this one broke"; add unfailed parts from the same batch and it becomes "this is where the batch deviates". That saves more money than any packaging material.

Write transit damage into the report instead of hiding it. Hiding it swaps the object of analysis. The conclusion looks clean while the corrective action goes the wrong way. Reporting it separately is a mark of competence, not of carelessness.

A packaging record is the only thing that can speak for you in a dispute. An unboxing video, a humidity indicator and a weighing slip take under ten minutes together and decide whether a report still stands six months later.

Where the part came off a vehicle, the gap between installed and tested state is a variable in itself, and the four gaps in the test passed but the vehicle still failed are worth checking against. Judgement of the material itself belongs to materials and structure testing and is a different task from reading a fracture.

Scheduling is arranged per project; you can state your expected delivery date when submitting samples, and we will confirm a feasible plan against the current schedule and report progress at each milestone.

Related Q&A

Related questions

Frequently asked questions on the same topic. The first paragraph of each answer is the conclusion.

Should a failed part be cleaned before it is shipped?
No. The residue on the part is evidence in itself: flux residue, ionic contamination, corrosion products, leached plasticiser and debris near the fracture all have to be recorded in their original state. Cleaning removes two things at once, the soluble contamination and the particles attached to the fracture surface, and those are exactly the clues that point to where failure started and what medium was involved. If cleaning is required, do it inside the analysis flow, record first and clean afterwards, and keep one uncleaned reference part. Results from cleaned and uncleaned parts of the same batch cannot be compared directly.
Can a failed part be wrapped in ordinary bubble wrap?
It depends on which area is being wrapped. Bubble wrap is fine on a housing, but fracture faces, terminal contact areas, gold surfaces and plated surfaces must not touch any material at all. Bubble wrap pressed onto a fracture leaves compaction marks and parallel scratches that ruin the reading of dimples and cleavage patterns. The correct approach is to suspend the fracture: locate the part inside a rigid box, leave the fracture side free, or support the part on a non-functional area. Static-sensitive devices also need a metallised shielding bag with pins shorted; a plain zip bag keeps out dust and nothing else.
Can a failed part shipped in winter be opened as soon as it arrives?
No. Let it reach room temperature first. A cold part brought indoors condenses moisture immediately, on the part surface and on the inside of the packaging, and that condensation creates fresh corrosion marks and leakage paths that mix with the original failure. Keep the part in its outer packaging until it is close to ambient temperature, photograph the outer packaging and the humidity indicator before opening, then photograph each layer from outside in. The same rule applies in the rainy season and on long routes. Desiccant and a humidity indicator inside the packaging are the record of whether moisture got in on the way.

These answers share the same data source as the FAQ page.

Have a testing requirement? Send us your product details

Tell us the product model and test requirements. Our engineers will map out the test plan, the applicable standards and the item combination, and provide a quotation reference. The more specific the request, the sharper the answer.

  • Free scoping of the test plan and standards
  • Pre-scan testing during R&D to cut rework cost
  • On-site visits and witnessed testing supported
  • Scheduling per project, with progress updates at each milestone

Received — we will contact you shortly and follow up with a test plan and quotation.

By submitting you agree to be contacted by phone or email. Scheduling follows the project’s actual availability and is subject to mutual confirmation.

13510907826
Call