Skip to main content
  1. Home
  2. Technical Blog
  3. Materials & Chemistry
  4. Chemical Resistance Test Passed, Part Cracked Later - Plastic Stress Cracking Needs Three Conditions at Once

Chemical Resistance Test Passed, Part Cracked Later - Plastic Stress Cracking Needs Three Conditions at Once

Key takeaways

A chemical resistance test runs unloaded, so it can only answer whether material and medium are compatible; stress cracking needs residual stress, medium and time-temperature together. The four sources of residual stress are gate and flow orientation, wall-thickness steps, demolding and ejection, and assembly preload or secondary operations, and each leaves a locatable signature. The medium does not corrode the part - it lowers the threshold for cracking, so "no visible deformation after soaking" is not a criterion. Evaluate with specimens under a known strain and read initiation time and critical stress, and separate fracture types by origin, plastic deformation and crack pattern. Relieve stress first, then discuss another grade or another material.

A chemical resistance soak that passed, followed by a part that cracked months later, is not a contradiction. Stress cracking in plastics needs three conditions at the same time: residual stress left by moulding, a medium able to enter the surface, and enough contact time at temperature. A conventional chemical resistance test supplies the medium but not the stress - it answers half the question.

The conclusion usually heard on the floor is "this material cannot handle the cleaning agent". Put the cracked part under polarised light and the crack sits exactly opposite the gate, where the fringe bands are dense enough to shine. The medium did not change, the grade did not change; what changed is the stress at that location.

1. Why a chemical resistance test cannot catch stress cracking

Most chemical resistance clauses follow one skeleton: the part or a coupon contacts a specified medium, stays at a specified temperature for a specified time, and is then checked for appearance, dimensions, mass and performance (both GB/T 28046 and ISO 16750 are built this way).

There is no loading step in that skeleton. The sample carries no working load, and preserving moulded-in stress is not a requirement. Flat coupons are often cut from finished parts, which releases part of the stress before the test even starts.

A real part is different:

  • It leaves the mould carrying residual stress, higher near the gate and at the end of flow;
  • Assembly adds preload: interference at snap fits, hoop stress from thread-forming screws, press fits and inserts;
  • Some locations work near yield for years without showing visible deformation.
ItemConventional chemical resistance testStress cracking evaluation
---------
Stress state of sampleNo applied stress, residual stress not controlledKnown constant strain or stress applied
FocusMedium type, temperature, duration, appearance and propertiesStress-time combination at which cracking starts
What the result readsWhether this material survives this mediumHow far this stress level lowers the threshold

In one line: chemical resistance answers "compatible or not", stress cracking answers "how much stress can it still carry". The first is material screening, the second is a structural verdict. Neither report substitutes for the other.

2. Where residual stress comes from: four sources, all locatable

Residual stress is not an abstraction; it has a location on the part. Checking these four places is more useful than arguing about grades.

Stress sourceWhere it shows on the partField signatureMitigation
------------
Gate and flow orientationOpposite the gate, end of flow, weld linesDense fringes, crack aligned with gate positionMove or add gates, lower injection speed and packing
Wall-thickness stepThick-to-thin transition, rib roots, boss rootsSink mark and crack in the same placeEven out wall thickness, add transition radii
Demolding and ejectionAround ejector marks, deep side wallsEjector whitening, local gloss, light scuffingMore draft, adjusted ejection force and mould temperature
Assembly preload and secondary operationsSnap-fit roots, screw bosses, ultrasonic weld lines, insert perimetersWhitening right after assemblyReduce interference, redesign bosses, keep weld lines off load paths

The first two come from moulding, the last two from assembly and secondary operations. Same mould, same grade, only the assembly method changed and the part stopped cracking - which means the variable was never the material. Most cracking disputes on interior and exterior parts, the kind handled under interior and exterior component testing, end up in one of these four rows that nobody recorded.

One more item is easily missed: annealing or drying changes dimensions, especially on hygroscopic materials. Relieving stress by annealing is not a free action - dimensions and assembly force have to be re-measured afterwards.

3. The medium does not corrode, it lowers the cracking threshold

The mechanism is simple. The medium enters the surface, lowers surface energy, and makes crazes open more easily. Crazes joining up become a crack.

None of this requires a measurable mass change or visible swelling. So "no deformation and no discolouration after soaking" is not a criterion - both are clean in the early stage of cracking.

Three families of media behave very differently:

Medium familyHow it actsWhere it appearsWhat to watch
------------
Solvent type (alcohols, ketones, esters, cleaners)Swells and lowers surface energy, acts fastAssembly cleaning, label adhesive, pre-coating wipeWhitening or tackiness after soak, cracking from edges
Surfactant type (detergents, hand sanitiser, sunscreen)Enters craze tips, acts slowly at a low thresholdDaily wiping and handling of interior partsNothing short term, cracking after repeated contact
Oils and working fluids (fuel, engine oil, coolant, urea)Acts together with temperature, locally concentratedEngine bay, underbody, around filler necksInvisible at room temperature, appears once heated

Two media appear on no reagent list at all: residues of release agent and cleaning solvent (on the part, not on the list), and assembly consumables such as threadlocker and sealant. Anaerobic threadlockers bring out stress cracking more readily on amorphous materials, and they are usually chosen by the assembly plant without telling the material side.

Time and temperature have to be written together. The same medium shows nothing at room temperature and acts quickly once heated; conversely, lower the stress level and the tolerable time lengthens. It is one simultaneous condition - reading any single term alone gives a wrong conclusion.

The reagent list itself is set by mounting location and is covered separately (how chemical load is tested), so it is not repeated here.

4. How to catch it before the small batch

Three steps, in order.

First, a stressed specimen. Apply a known constant strain to a specimen - a bending rig or four-point loading as in the ISO 22088 family for environmental stress cracking - and immerse it in the target medium. Read initiation time and critical stress, not appearance after the soak. Only numbers obtained this way can be compared with the stress values from structural simulation.

Second, map the stress before choosing test points. Inspect moulded parts under polarised light and look at fringe density; dense bands mark the candidate crack sites. Write those locations into the test plan instead of cutting a random flat coupon - a coupon whose result does not match the part is a common waste in this kind of evaluation.

Third, read the fracture surface. The three failure types differ enough to separate:

FeatureStress crackingOverloadThermal stress cracking
------------
OriginSurface, at a stress concentrationMid-section or at a defectWall step, around inserts
Plastic deformationAlmost noneWhitening, elongation, neckingSlight
Crack patternSeveral parallel fine cracks along stressOne dominant fast crackAlong thermal gradient or weld line
TriggerMedium plus residual stress plus timeSingle overload eventThermal cycling, uneven cooling

One supporting check: put uncracked parts from the same batch under polarised light. If dense fringes coincide with the crack site, the cause is residual stress, not a wrong choice of medium.

5. Corrective sequence: relieve stress first, then discuss material

Get the order wrong and every step is paid for twice.

Locate the initiation site, identify the stress source there, then relieve it: adjust gate position and injection parameters, even out wall thickness, add transition radii, reduce interference and boss hoop stress, anneal where needed. After this, most parts stop cracking.

Only if that is not enough does a grade or material change come in. The cost has to be stated up front: shrinkage differences require mould changes, environmental and chemical tests are repeated, and approval documents are revised. And if the stress source is untouched, the crack often reappears in the same place after the switch - by then the money is spent.

One rule: change structure before process, change process before material. Annealing and parameter tuning are process, gate and wall changes are structure, a grade change is material - walking up that staircase, cost increases at every step.

6. A few plain words

State three things when submitting samples: how the part is moulded (gate position, whether it is annealed), where it is mounted, and what it will contact. Those three decide which stress rig is used, which medium is applied, and which quantity is read. Miss one and the laboratory can only run a conventional chemical resistance test, and the report will not answer your question.

A chemical resistance report and a stress cracking evaluation are two different documents. When an OEM reviews a report it asks "will this location crack", not "does the material resist this reagent". Answer the wrong question and the report will not clear review however tidy it looks.

At TMC LAB this kind of commission starts by fixing the loading and medium combination from the initiation site and the assembly method, and the verdict is written as comparable quantities - initiation time, critical stress - rather than "no abnormality". Compression set and media swelling on the seal side are a separate chain (why seals leak); elastomers and rigid plastics are judged differently and should not be mixed. Routine material testing and the failure analysis route are set out under material testing.

Scheduling is arranged per project; you can state your expected delivery date when submitting samples, and we will confirm a feasible plan against the current schedule and report progress at each milestone.

Related Q&A

Related questions

Frequently asked questions on the same topic. The first paragraph of each answer is the conclusion.

The chemical resistance test passed but the part cracked in service - was the test wrong?
Usually the test was not wrong; the two tests answer different questions. A chemical resistance test runs on unloaded specimens and reads whether the material and the specified medium are compatible at a given temperature and duration. A part that cracks in service still carries molded-in residual stress plus assembly preload, and once the medium enters the surface the threshold for cracking drops, so it fails well below yield. Covering that case needs a separate stress-cracking evaluation with specimens under a known strain - a bending or four-point rig - reading initiation time and critical stress, rather than extending the soak time of the chemical test.
A plastic part cracked - how do I separate stress cracking from overload?
Check three things. Origin: stress cracking starts at a surface, usually at a stress concentration, while overload starts mid-section or at a defect. Plastic deformation: stress cracking leaves almost no macroscopic deformation and a fine, flat fracture surface, whereas overload shows whitening, elongation and necking. Crack pattern: stress cracking usually presents several parallel fine cracks advancing along the stress direction, while overload is one dominant crack running fast. One more piece of evidence - inspect uncracked parts from the same batch under polarised light; if dense fringe bands coincide with the crack site, residual stress is the driver.
Will switching to a more chemical-resistant plastic grade solve it?
Not necessarily, and doing it first costs more. The crack location is set by stress; another grade does not move the stress source, and many parts crack again in the same place after the switch. The workable order is to locate the initiation site, identify the stress source there, then relieve it - adjust gate position and injection parameters, even out wall thickness, add transition radii, reduce interference and boss hoop stress, and anneal where needed. Only if that is not enough does a grade or material change come in, and then mould modification from shrinkage differences plus repeated environmental and chemical testing come with it.

These answers share the same data source as the FAQ page.

Have a testing requirement? Send us your product details

Tell us the product model and test requirements. Our engineers will map out the test plan, the applicable standards and the item combination, and provide a quotation reference. The more specific the request, the sharper the answer.

  • Free scoping of the test plan and standards
  • Pre-scan testing during R&D to cut rework cost
  • On-site visits and witnessed testing supported
  • Scheduling per project, with progress updates at each milestone

Received — we will contact you shortly and follow up with a test plan and quotation.

By submitting you agree to be contacted by phone or email. Scheduling follows the project’s actual availability and is subject to mutual confirmation.

13510907826
Call