Key takeaways

Sort a bend crack by location first: an origin at the burr side of the blanked edge points to blanking quality, a crack running the full length of the bend line points to rolling direction, and a rough or peeling outer surface points to a tight radius and grain condition. The four zones of a blanked edge - rollover, burnish, fracture, burr - exist before bending, and the fracture zone plus the burr are notches; put a notch on the tension side of the outer radius and it starts a crack. If the same sheet stops cracking when the nesting direction changes, the problem is fibre direction, not grade. The radius-to-thickness ratio sets the surface strain on the outer fibre, so thick stock with a tight radius is inherently harder to form. Burr-in is mechanics behind a shop-floor habit, not a matter of preference.

A bend that cracks along the outer radius usually triggers one reaction: blame the material grade, or blame the supplier for changing it. Work through failed parts one by one and three things turn out to decide whether it cracks, and all three were fixed at tooling and nesting: the quality of the blanked edge, the angle between the bend line and the rolling direction, and the ratio of bend radius to sheet thickness. Changing material addresses one of the three and leaves the other two untouched.

This article is about forming cracks in the sheet-metal part itself - terminals, shields, brackets, busbars, enclosures. Coating cracks at a bend are a different failure with its own criterion at the interface, taken apart separately (plating adhesion, blistering and peeling).

1. Read the crack location first: three positions, three causes

Do not start with metallography. Look at where the crack starts and which way it runs; that step alone removes most of the search space.

An origin on the blanked edge, especially on the burr side, points to blanking quality. A crack running the full width of the bend line points to rolling direction. A crack confined to the outer surface, fine and net-like or flaking, points to a tight radius and the condition of the outer grains. The corrective action differs completely between the three, and applying the wrong one changes nothing.

LocationWhat it indicatesWhat to check next
---------
Starts at the blanked edge or burr side, runs diagonally into the bodyA notch on the tension side started itEdge photos of unbent parts from the same batch
Runs the full length of the bend lineTension direction fell across the sheetRolling direction versus bend line on the nesting drawing
Outer surface rough, flaking, fine network of cracksSurface strain exceeded ductilityActual radius, thickness tolerance, grain condition

2. Four zones on a blanked edge: the crack origin is set before bending

Blanking is not a clean cut. From top to bottom the edge runs through rollover, burnish, fracture and burr. Rollover is the rounded lip pulled down as the punch enters; burnish is the sheared face and the smoothest part; fracture is the rough torn face, itself a field of micro-cracks; the burr is the sliver pushed out at the end and is a sharp notch.

ZoneRole during bendingWhat it looks like when abnormal
---------
RolloverThins the edge, reduces load-bearing sectionExcessive rollover leaves too little effective thickness
BurnishFlat face with low notch sensitivityToo small a share means incomplete shearing
FractureRough torn face, a micro-crack starterToo large a share, and the crack starts here
BurrSharp notch with high stress concentrationTall burr opens as soon as it is on the tension side

The proportions of those four zones are set by die clearance, edge wear and material condition, not by the grade on the certificate. Wider clearance raises the fracture and burr share. A worn edge makes the burr taller and thicker. Harder stock or severe work hardening narrows the burnish band. So the same drawing on the same press, with a worn or freshly reground tool set, can step the crack rate up.

That explains the common confusion: a new material batch arrives and parts still crack in the same place. The origin is a notch, not insufficient strength. With the notch present, higher strength still starts from the notch.

The check is simple: take unbent parts from the same batch, photograph the edge, measure the share of fracture zone and burr. The edge tells you before the part cracks.

3. Bend line versus rolling direction: the same sheet stops cracking when the nesting changes

Rolling elongates inclusions and grains along the rolling direction, so sheet is anisotropic: ductility is better along the rolling direction than across it. During bending the outer fibre is in tension perpendicular to the bend line, so the angle between the bend line and the rolling direction decides whether the outer fibre is stretched along the grain or across it.

Bend line versus rolling directionTension direction on the outer fibreTendency and nesting practice
---------
PerpendicularAlong the rolling direction, good ductilityLow cracking tendency, preferred in nesting
ObliqueSomewhere in betweenDepends on angle and radius, verify by measurement
ParallelAcross the sheet, poor ductilityHigh cracking tendency, change nesting or radius

The engineering practice is not complicated: mark the rolling direction on the nesting drawing and keep bend lines perpendicular to it. The difficulty is that incoming sheet is often unmarked, or the marking is inconsistent between batches.

The check: separate cracked from sound parts and go back to the nesting drawing to see whether their bend line orientations differ. If every cracked part sits on the same nesting orientation, the answer is there and the material file can stay closed.

One more layer is often missed: a part with several bends can have bend lines in different orientations, so one bend cracks and another does not. That gets misread as a problem with one station of the tool.

4. Bend radius and thickness: one ratio on the drawing

Bend radius is not a cosmetic dimension. The tighter the radius, the higher the tensile strain on the outer surface; once the strain exceeds ductility in that direction, the surface flakes, then shows fine cracks, then goes through.

Thickness enters the same ratio. Thicker stock pushes the neutral axis outward, so at the same radius the outer fibre sees more strain. "This radius has been fine for years in thin stock, and cracks as soon as we go thicker" is therefore expected, not a sign that the material got worse.

ChangeOuter-fibre strainWhat shows up
---------
Smaller radius, including tool wearHigherFlaking and fine cracks, cracked parts concentrated at tight radii
Greater thickness, including tolerance limitHigherThick parts crack first, thin parts are fine
Over-bend then corrected backSecond loadingA work-hardened outer fibre is pulled again, and cracks on the correction

Springback deserves its own note. Springback is unavoidable, and shops commonly over-bend and then correct to hit the angle. That correction loads an already work-hardened outer fibre a second time. The part survives the first bend and cracks on the correction, while the record shows one bend.

The checks: measure the actual radius with a gauge instead of copying the drawing; re-check parts at the upper thickness tolerance; and ask whether over-bend and correction is part of the route.

5. Burr orientation: the mechanics behind a shop-floor habit

A burr is a notch, and a notch does not belong on the tension face. Bending puts the outer fibre in tension and the inner fibre in compression, so the burr faces inward, toward the compression side. The habit is mechanics, not preference.

Inward is not free of cost: compression collapses the burr and can print a mark, affecting the mating face, appearance and downstream plating. So there are two criteria, not one.

Burr positionConsequencePractice
---------
Outward, on the tension sideNotch on the tension face, cracks at the bendChange nesting or flip the blank, not a die adjustment
Inward, on the compression sideCollapse can print a markDecide deburring or chamfering by appearance and assembly needs
DeburredNotch removed, edge slightly thinnedDeburring needs a consistent acceptance criterion

That column belongs in the drawing. Left to habit, it flips when the line or the shift changes.

6. Submission and judgement: five columns on the drawing or the request

Most disputes about these parts are not technical. The drawing gives shape and omits forming conditions. Miss one of the five columns below and the conclusion becomes hard to reproduce.

ColumnWhat it statesWhat is lost without it
---------
Material and rolling directionGrade, temper, batch, rolling mark on incoming sheetBatch and orientation changes go unnoticed, the problem repeats
Edge qualityAcceptance criterion for fracture zone and burr shareYou learn the edge is bad only after parts crack
Bend line orientationRolling direction and each bend angle marked on the nesting drawingBends behave differently on one part, root cause cannot be assigned
Radius and thicknessActual radius, thickness tolerance, whether over-bend is allowedThe crack happens on the correction while the record shows one bend
Burr conditionOrientation, deburring, acceptance methodDirection follows the line, marks and cracks alternate

Judgement needs a clean split. Forming practice belongs to the drawing and the process file; standards do not cover it. Standards provide the applied conditions and the pass classification - for example the mechanical load clauses in GB/T 28046 and the ISO 16750 series define how vibration and shock are applied and how functional status is judged, but not what bend radius your part should use or how tall a burr may be.

Micro-cracks that already exist will grow through later mechanical load, temperature cycling and assembly. So the order is forming first, testing second: a test amplifies an existing notch, it does not remove one. For the measurement side of mechanical properties see material mechanical testing; for parts that have already cracked, fracture and metallographic work runs through failure analysis.

Assembly often joins in: a part forced into place, a bolt pulled up hard, a bracket bent to align. When those forces share a direction with bending residual stress, the crack appears after assembly rather than on the press, a path covered in assembly stress and pre-spent life. Board level has a parallel case - a ceramic capacitor that cracks after a small board flex, different mechanism, same way of thinking (flex cracks versus thermal cracks).

When TMC LAB examines parts like these, three things are asked for first: unbent flat parts from the same batch, a nesting drawing with the rolling direction marked, and the edge photographs quality control already holds. With those three, most parts can be assigned a direction without any instrument.

7. A few plain words

With bend cracks, sequence matters more than equipment. Look at the edge, then at the nesting orientation, then measure the actual radius. None of the three costs money, and together they keep most parts from being re-run through a material change.

Material is the last move, because it addresses one of three factors and is the expensive one: new material approval, new scheduling, new validation.

Do not bend a cracked part back to look at it. Once the fracture is opened a second time, the origin and propagation direction are gone, and what remains is guesswork.

Scheduling is arranged per project; you can state your expected delivery date when submitting samples, and we will confirm a feasible plan against the current schedule and report progress at each milestone.

Related Q&A

Related questions

Frequently asked questions on the same topic. The first paragraph of each answer is the conclusion.

Why do some parts from the same sheet crack at the bend while others do not?
Look at the nesting direction first. During bending the outer fibre is in tension perpendicular to the bend line. If parts from the same sheet are cut with different nesting orientations, the angle between the bend line and the rolling direction differs, and a part whose tension direction falls along the rolling direction has better ductility than one loaded across it. Then look at the blanked edge: die clearance and edge wear vary across a tool, so the share of fracture zone and burr varies too. Finally check the actual bend radius and the sheet thickness - a worn tool reduces the radius and stock at the upper thickness tolerance adds strain, and the two together land on the cracking side. All three can be investigated without changing material or running a chamber.
If a bend cracks, is changing the material the first move?
It addresses one of the three factors, and often not the dominant one. Do three things that cost nothing first: take an unbent part from the same batch and inspect the blanked edge, measuring the share of fracture zone and burr; mark the rolling direction on the nesting drawing and check the angle to the bend line; measure the actual radius with a radius gauge and re-check a part at the upper thickness tolerance. Only when all three are normal does the material grade, temper and batch become the conversation. If the edge is already rough with tall burrs, any material will crack in the same place, because the crack starts at a notch, not at insufficient strength.
Should the burr face inward or outward when bending?
Inward, toward the compression side. During bending the outer fibre is in tension and the inner fibre in compression, and a burr is a notch; a notch must not sit on the tension face, or the part starts with a crack line already open. Inward is not free of cost: compression collapses the burr, which can print a mark and affect fit, appearance or downstream plating. So there are two criteria - no notch on the tension side, and burrs tolerated on the compression side but judged against appearance and assembly requirements for deburring or chamfering. Put that column in the drawing rather than leaving it to shop-floor habit.

These answers share the same data source as the FAQ page.

Have a testing requirement? Send us your product details

Tell us the product model and test requirements. Our engineers will map out the test plan, the applicable standards and the item combination, and provide a quotation reference. The more specific the request, the sharper the answer.

  • Free scoping of the test plan and standards
  • Pre-scan testing during R&D to cut rework cost
  • On-site visits and witnessed testing supported
  • Scheduling per project, with progress updates at each milestone

Received — we will contact you shortly and follow up with a test plan and quotation.

By submitting you agree to be contacted by phone or email. Scheduling follows the project’s actual availability and is subject to mutual confirmation.