Skip to main content
  1. Home
  2. Technical Blog
  3. Failure Analysis
  4. A Cracked MLCC Is Not Always a Supplier Issue - Flex Cracks and Thermal Cracks Start in Different Places

A Cracked MLCC Is Not Always a Supplier Issue - Flex Cracks and Thermal Cracks Start in Different Places

Key takeaways

A cracked MLCC is not one failure but two. A flex crack enters obliquely from the terminal-to-body junction, appears after assembly, and is fixed at depanelling, screw torque and connector insertion force. A thermal crack starts vertically at the solder fillet, exists right after reflow, and is fixed in the reflow profile and touch-up rules. The criterion is not whether a crack exists, but where it starts on the cross section, whether the reference designators cluster or scatter, and whether the first article after soldering already had it. Capacitance and insulation resistance can both read normal before the crack goes through, so a passed measurement is not evidence of no crack.

When an MLCC cracks, the first question is usually whether the lot is bad. What actually decides the corrective action is where the crack starts: entering obliquely from the junction between termination and ceramic body means the board was bent, while running vertically from the solder fillet at the termination means the soldering thermal excursion was too abrupt. The two sit in different places on the cross section, appear at different points in the process, and are fixed in opposite directions - one by process, one by layout and pad design.

1. Two cracks, two different origins

A ceramic capacitor is a brittle part: strong in compression, weak in tension, with almost no plastic deformation. Mounted on a board, two stress paths can break it, and they break it differently.

A flex crack starts at the junction between termination and ceramic body, on the board side. When the board bends, the solder joint holds the termination while the body follows the board, concentrating tensile stress at the junction. The crack enters the body obliquely and a single bending event often produces a diagonal crack running through both ends.

A thermal crack starts at the root of the solder fillet at the termination and runs closer to perpendicular to the board surface. It relates to the thermal gradient of the soldering process: the joint cools quickly, the termination is metal and conducts heat quickly, the ceramic body conducts slowly, the two shrink differently, and the stress releases along the interface, following the internal electrode layers.

CriterionFlex crackThermal crack
---------
OriginTermination-to-body junction, board sideRoot of solder fillet, along the interface
DirectionOblique into the body, often through both endsNear perpendicular to the board, may stop part way
Cross-section appearanceMostly transgranular, brighter fractureDelamination along internal electrodes, stepped
DistributionClustered at board edges, screw holes, depanelling lines, connector force directionWeakly related to designator position, strongly related to board thickness, pad and reflow profile
Point in processAfter assembly operationsPresent right after soldering, grows with thermal cycling

Table basis: these are general morphology criteria used in failure analysis; the actual call rests on the measured cross section and the customer technical agreement.

In one line: a flex crack is created when the board is bent during assembly, a thermal crack is created when soldering heats it too abruptly.

2. Bench tests miss it because an early crack does not change electrical parameters

This is where this failure mode slips through.

Before a crack goes through both electrode layers, the electrodes remain in parallel, the capacitance shift falls inside measurement repeatability, and nothing can be read. Insulation resistance only drops clearly after the crack has taken up moisture and a conductive path has grown. So in-circuit test passes, burn-in passes, and the failure shows up in the vehicle - not because testing was careless, but because the quantities measured are not sensitive to this defect.

A passed measurement proves the crack had not gone through at that moment. It is not evidence that no crack exists.

Two routes can force it out. The physical route is cross sectioning and polishing to see the origin, or acoustic scanning to see internal delamination; the first is conclusive but destroys the sample, the second is non-destructive but can miss very fine cracks. The stress route is to let differential expansion open the crack through temperature cycling, then let moisture in through damp heat while monitoring insulation resistance for a step drop. This is the same condition design as any environmental test, with the criterion changed from "function normal" to "did insulation fall".

One caution: if the symptom is leakage or falling insulation resistance, do not jump straight to a capacitor crack. Surface contamination and electrochemical migration take a different path; if the three conditions of ion contamination, water film and bias in electrochemical migration do not line up, come back to cracking.

3. Where mechanical stress comes from: check these five operations first

Flex cracks almost always map back to a step in the process.

OperationHow stress arisesWhere the crack lands
---------
DepanellingV-cut snapping, router push, manual breakingDesignators near the depanelling line
Screw fixingUneven torque, missing washer, forced alignment across holesA ring around the screw hole
Connector insertionInsertion force lands on the joints, board is pushed into bendingCapacitors behind and beside the connector
Heatsink or shield pressingUneven pressing face, over-thick gap pad, off-centre loadUnder and around the pressed area
Handling and test fixturesToo few supports, pusher pins right above componentsNear the fixture contact points

The work is to map each operation onto the positional distribution of cracked designators: a column at the board edge points to depanelling, a ring around a screw hole points to torque and tightening order, a cluster behind a connector points to insertion force.

One geometric factor is often missed: the span between the two terminations. The larger the span, the greater the height difference between the ends when the board bends, and the greater the strain difference across the part. Layout therefore has to consider both distance from the stress source and the direction of the part's long axis relative to the bend. Moving a large capacitor slightly away from the edge while its long axis points straight into the bending direction usually achieves little.

4. Thermal stress: not how hot, but how fast

The input for a thermal crack is not the peak reflow temperature; it is the rate of change and the mismatch across the interface.

Thermal mass difference between termination and body. The termination is metal and heats and cools quickly; the ceramic body conducts slowly. On the same reflow profile the two experience different histories, and shear appears at the interface.

Cooling rate. Everyone watches the ramp up; the ramp down is often ignored. Cool too fast and the joint and termination carry a larger shrinkage mismatch while still relatively soft.

Touch-up soldering. An iron pressed directly on the termination raises local temperature instantly. The more touch-ups and the longer each dwell, the more thermal shock the interface sees. This is extremely common at rework stations, and rework records rarely enter the failure analysis.

Board thickness and copper area. Thick boards with large copper pours dissipate heat quickly and cool locally faster; larger parts develop a larger internal gradient.

To judge a thermal crack, pull the reflow profile and the rework records together, rather than only checking whether the oven setpoints look right.

5. How to prove which one it is

Three comparisons, and a conclusion is weak if any one is missing.

First, look at the origin on the cross section. Does the crack start obliquely at the termination-to-body junction, or vertically at the fillet root; is it transgranular, or delamination along internal electrodes. This is direct evidence, and the grinding and polishing route is the same as in terminal cross-section analysis.

Second, look at clustering in the designator map. Plot the failed designators on the board drawing: do they cluster around geometric features such as edges, holes and depanelling lines, or scatter randomly. Clustering points to mechanical stress, scattering points to incoming material or thermal. This step is non-destructive and gives a high return.

Third, align the timeline. Sample the first article after soldering for observation or scanning to establish a baseline, then sample again after assembly. Present right after soldering means thermal; appearing only after assembly means mechanical. Without that baseline, every later inference stays an inference.

One clarification: delamination and cracking on the same board are different things. PCBA delamination and popcorn is interfacial separation between laminate and copper under moisture plus fast heating - a board issue. This article is about cracking of the ceramic body itself - a component issue. The cross-section appearance and the corrective direction do not carry over, so do not merge the two in a report.

6. Outline and corrective action: what changes at each level

LevelActionWhere to start
---------
Part selectionSoft termination, higher flex rating, smaller case sizeDesignators at board edges, screw holes and connector force direction first
LayoutKeep away from depanelling lines and holes, clear of pressed areas, control span and orientationThe parts aligned with the stress direction first
ProcessDepanelling method, screw torque and tightening order, washers, touch-up rules and limitsDepanelling and screws first, then rework
VerificationTemperature cycling to open the crack, damp heat to admit moisture, insulation monitored during exposureMatched one-to-one to the identified failure chain

Of the four, part selection adds margin while process and layout reduce the input. Changing the part without changing the process consumes the margin; the problem is postponed, not removed.

For test planning, the logic of tailoring by mounting location and grouping by failure chain in the automotive environmental reliability test checklist applies directly. On the materials side, mechanical items such as bending, peel and thermal shock under materials and processes are complementary, not a substitute - they test the board and joint resistance, not cracking of the component body. At the standards level, the framework for test methods and severity classes is in GB/T 28046 and ISO 16750; specific clauses follow the customer's controlled version.

A few plain words

First, changing suppliers does not fix board bending. A certificate of conformance and "no crack after assembly" are two different things, and the former does not cover the latter.

Second, a failure report that says "capacitor cracked" without cross-section morphology, without a designator map, and without a post-solder baseline gives a conclusion, not evidence. Negotiating with a supplier on that conclusion goes nowhere.

Third, the recommended order is: look at the distribution, determine the type, change process and layout, and put part selection after that. Done the other way round, the usual outcome is two rounds of part changes with the crack still in the same place.

TMC LAB asks for the designator map, the process timeline and the rework records together before deciding which part to section - because sectioning the wrong one points the corrective action in exactly the opposite direction. If the symptom is intermittent functional anomaly rather than leakage, the diagnostic path differs; start with the reproduction sequence for intermittent failures.

Scheduling is arranged per project; you can state your expected delivery date when submitting samples, and we will confirm a feasible plan against the current schedule and report progress at each milestone.

Related Q&A

Related questions

Frequently asked questions on the same topic. The first paragraph of each answer is the conclusion.

If capacitance reads normal, does that mean the MLCC is not cracked?
No. Before a crack goes through, the internal electrodes are still in parallel, so the capacitance shift falls inside measurement repeatability and cannot be read out. Insulation resistance only drops after the crack has taken up moisture and a conductive path has grown. This is why boards can pass in-circuit test and burn-in and still fail in the vehicle. Whether a crack exists is decided by physical means - cross sectioning, acoustic scanning - or by driving it out with temperature cycling plus damp heat and re-measuring. An out-of-spec electrical reading only proves the crack already went through; it says nothing about where it started.
Is a cracked MLCC always an incoming material problem from the capacitor supplier?
Usually not. The ceramic body is brittle, strong in compression and weak in tension, with almost no plastic deformation, which makes it highly sensitive to board bending, screw torque and connector insertion force. Cracks present in incoming parts - poor termination sintering, micro-cracks from cutting - do exist, but they tend to appear across multiple designators, multiple panels and often multiple assembly sites in the same lot. Assembly-induced cracks carry a strong positional signature, clustering at board edges, around screw holes, along depanelling lines and in the direction of connector force. Comparing the two distributions tells you more than any supplier statement. To argue incoming material, rule out the process first, not the other way round.
Does switching to soft-termination MLCCs solve cracking completely?
Soft termination adds a conductive elastic layer between the termination and the ceramic body, which shaves the peak of the bending stress and is genuinely effective against flex cracks - hence its common use near board edges, around screw holes and on large boards. But it changes two things it cannot: it does not address thermal cracks, because that stress runs through the termination-to-solder interface and an elastic layer does not alter the thermal gradient of the soldering process; and it only raises margin, it does not remove stress, so a board bent hard enough will still crack. Part selection adds margin while process and layout reduce the input. Both directions have to move; changing the part alone usually postpones the problem.

These answers share the same data source as the FAQ page.

Have a testing requirement? Send us your product details

Tell us the product model and test requirements. Our engineers will map out the test plan, the applicable standards and the item combination, and provide a quotation reference. The more specific the request, the sharper the answer.

  • Free scoping of the test plan and standards
  • Pre-scan testing during R&D to cut rework cost
  • On-site visits and witnessed testing supported
  • Scheduling per project, with progress updates at each milestone

Received — we will contact you shortly and follow up with a test plan and quotation.

By submitting you agree to be contacted by phone or email. Scheduling follows the project’s actual availability and is subject to mutual confirmation.

13510907826
Call