Skip to main content
  1. Home
  2. Technical Blog
  3. Materials & Chemistry
  4. The Pull-Off Passed but Fatigue Started in the Heat-Affected Zone - Welding Changes the Metal Beside the Joint

The Pull-Off Passed but Fatigue Started in the Heat-Affected Zone - Welding Changes the Metal Beside the Joint

Key takeaways

Cut a fusion-welded joint across and there are only three regions - nugget, heat-affected zone, base metal - similar in composition, very different in state. A fracture in the heat-affected zone says the grain structure, softening or hardening and residual stress in that ring are now weaker than the base metal, so the corrective route runs through heat input, cooling and the original condition of the base metal; a fracture in the base metal is a good sign. Heat input is not a parameter but a ratio of power to travel speed (or weld time in resistance spot welding), and current enters squared in spot welding, so it moves results faster than expected. The zone holds at least four bands - coarse grain, fine grain, partially transformed and tempered-softened - while aluminium has no phase change at all and reads as over-ageing softening that natural ageing after welding will not restore. A pull-off test is one static load: it answers whether one load is survivable and nothing else. Fracture appearance, nugget size, hardness traverse and fatigue have to be added, and the fracture location has to reach the report.

A passing pull-off result proves the joint survived one load. What fusion welding really changes is not the nugget itself but the ring of metal beside it, heated and cooled repeatedly, where grain structure, hardness and residual stress no longer match the base metal. When a fracture falls inside that ring, the failure location was set by the weld thermal cycle - and a pull-off number cannot show it.

The boundary first. This article covers metallurgical changes on both sides of the fusion line in fusion-welded joints - resistance spot welding, laser welding, arc welding - and how to read the fracture location. Soft soldering on board-level components, where the break sits in the intermetallic, the pad or the solder bulk, is a separate subject covered under the three fracture locations of a solder joint. Ultrasonic welding of plastics is a third, judged on interface fusion and melt depth, as described in plastic weld strength.

1. Where the fracture sits is already a conclusion

Cut a fusion-welded joint across and there are only three regions: the nugget that melted and solidified, the heat-affected zone that was heated but never melted, and the base metal that was never reached. Similar composition, very different state.

Fracture locationWhat it saysWhat to examine next
---------
Inside the nugget or at the fusion interfaceThe weld itself underperformed: undersized nugget, lack of fusion, porosity or hot crackingParameter window, electrode condition, surface cleanliness and coating
Heat-affected zoneStructure or residual stress in that ring is now weaker than the base metalHeat input, cooling rate, original condition of the base metal
Base metal, away from the fusion lineJoint strength exceeds the base metal; the weld is not the weak linkStructural design and the base metal itself

The last row is usually good news: the base metal broke first, so the joint did what it was supposed to do. That reading sits in direct conflict with how a pull-off value is used - the number only gives a magnitude, never a location.

The spread of fracture locations also back-calculates the process. A batch with a narrow strength distribution but two fracture modes means the window has drifted to its edge; a mix of interface tears and button pull-outs usually points to electrode wear or incoming surface condition.

2. Heat input sets how wide the ring is, and what it becomes

Heat input is not one parameter but a ratio of power to travel speed. Resistance spot welding has no travel speed, so weld time stands in - and the situation differs.

Which way heat input movesHow the zone respondsWhat it costs
---------
Higher (more power, slower travel)Wider, more grain growth, a more obvious softened bandMore distortion, lower toughness, wider residual stress field
Lower (less power, faster travel)Narrower, faster coolingHigher hardenability response in steel, more cold cracking risk
Spot welding: current too highNugget grows fast, expulsion and deeper indentationFaster electrode wear, indentation edge becomes a notch
Spot welding: current too lowUndersized nugget, fracture mode turns into an interface tearPull-off value may still pass

The spot-welding rows need separate treatment: current enters squared, the other two linearly. Move the current and the result moves faster than expected, which makes the real window narrower than it appears.

Indentation is easy to overlook. The electrode leaves a crater, its rim is a sharp corner in geometric terms, and that rim also marks the boundary of the heat-affected zone. Under vibration, cracks frequently start at that boundary rather than at the nugget centre.

3. The heat-affected zone is not one zone but at least three

In steel the zone can be split by peak temperature, each band with its own structure and properties.

BandWhere the peak temperature fallsCharacter
---------
Coarse-grain bandClose to the solidusClear grain growth, reduced toughness, a common site for brittle initiation
Fine-grain (recrystallised) bandJust above the austenitising temperatureEffectively one normalising pass; fine grains, strength and toughness usually adequate
Partially transformed bandBetween the two critical temperaturesNon-uniform, often banded structure, intermediate properties
Tempered soft bandBelow the transformation temperatureTempering in quenched and tempered steel, recrystallisation softening in cold-worked material

Aluminium replaces that whole table. There is no phase change, and the loss comes from coarsening of strengthening precipitates during the thermal cycle - over-ageing, not tempering. The consequence is practical: natural ageing after welding restores only the natural-ageing contribution, the lost peak strength does not return, and recovering it requires solution treatment and ageing on the whole part, which is rarely feasible once components are assembled.

Aluminium weld design therefore carries a joint efficiency margin that accounts for the softened band, instead of relying on a post-weld remedy.

4. Why a pull-off test cannot see any of this

A pull-off or lap-shear test is one static load. It answers whether the joint survives that load, and nothing about three other things: where it broke, how many cycles it will take, and whether it deformed first.

QuestionCan the pull-off answer itWhat to add
---------
Is one load survivableYesPull-off or lap shear, with fracture appearance recorded
Is the metallurgical bond adequateNoMetallographic section: nugget size, lack of fusion, porosity, hot cracks
Is that ring weakNoMicrohardness traverse across nugget, zone and base metal
Will it survive vehicle life in vibrationNoLap-shear fatigue, with crack initiation location recorded
How large is the residual stressNoX-ray diffraction or hole drilling, read together with restraint conditions

Fracture appearance belongs in the report; a single force value is not enough. A button pull-out and a flat tear along the interface are two different joints: in the first the nugget comes out intact from the base metal, in the second the joint separates along the fusion plane. Both can pass with the same number and mean opposite things.

Fatigue adds a stacking effect that is easy to miss. At the junction of fusion line and indentation rim, geometry provides a sharp corner, metallurgy provides a coarse-grain band, and mechanics adds weld residual tension. Three adverse conditions at one location, which is why that ring cracks first in vibration and thermal cycling - not by coincidence.

5. Two routine misreadings: galvanised steel and aluminium

In galvanised steel spot welding the problem often sits in the zinc, not the steel. Zinc boils far below the melting point of steel, so it vaporises first; when the vapour cannot escape it drives expulsion, leaves porosity and keeps the nugget from consolidating. Electrodes also pick up zinc, and once the face profile changes the current density at the next spot changes with it.

So a record reading "same line, same parameters, first spots fine, later spots tearing at the interface" should send you to electrode condition and dressing interval before parameters. "Per the process card" means nothing once the electrode has deformed.

Galvanised steel has another path that gets missed: at welding temperature zinc penetrates steel grain boundaries and causes liquid metal embrittlement. Cracks follow the boundaries, the macroscopic appearance often looks normal, and the fracture is brittle - easily misread as "the material is too brittle".

Aluminium runs the other way. High thermal conductivity drains heat fast, so more heat input is needed to form a nugget; a high expansion coefficient raises hot-cracking risk from solidification shrinkage; and the surface oxide melts far above the base metal, so an uncleaned surface will not weld through. Stacked together, the result is a wider, more severely softened zone - the same location has to be hot enough without becoming too hot.

6. Four techniques, combined so the verdict holds

Any single technique leaves a gap. The workable order: read the fracture appearance first, then section the joint to measure nugget and zone, then run a hardness traverse to locate and size the softened or hardened band, then use fatigue where cyclic behaviour has to be demonstrated.

ColumnWhat goes in itWhy it is often blank
---------
Base metal conditionGrade, supply condition (quenched and tempered, cold worked, aged), coating, thickness combinationGrade only, condition omitted
Method and parameter windowProcess, current or power range, force, weld or travel time, shielding gas"Per the process card"
Joint type and samplingLap or butt, thickness combination, which cut the specimen came from"Random from the batch"
CriterionForce value, fracture appearance, metallographic items, hardness traverseForce value only
RecordsParameter traces, scaled fracture photographs, hardness curves, micrographsOne page of pass/fail

The base metal condition column cannot be skipped. The same grade in quenched and tempered versus cold-worked condition is changed differently by the thermal cycle: tempering softening in one, recrystallisation softening in the other, at different locations and to different degrees. With grade alone, the report cannot be reproduced and two disagreeing results cannot be explained.

Keep the standards in their lanes. GB/T 28046 and ISO 16750 supply the applied conditions and functional status grading for mechanical and climatic loads - they specify what vibration and temperature cycling the part must endure, and say nothing about whether this particular weld was made well. Weld quality criteria live in a separate system: procedure qualification, spot-welding process specifications and destructive testing each have their own documents. Which one applies, and at which edition, follows the current edition and the customer technical agreement.

7. A few honest words

Fracture location is worth more than the force value. A passing batch that splits into two fracture modes has already drifted to the edge of its window - it just has not drifted far enough to generate a failing report.

Change the electrode, the coating, the thickness combination or the machine, and the conclusion has to be revisited. What changed is the ring of material, not the nugget.

One sentence worth keeping: welding does not leave the base metal with a seam, it leaves it with a ring of altered material. Static loading cannot see it; cyclic loading will find it for you.

Cracking on the outer arc of a bent part describes strain left in the part during forming; the four readings of a crimp cross-section describes interface quality in a different joint family. Three stages of one question: quality in joining and forming shows up first in where it breaks, and only then in the numbers.

TMC LAB sets base metal condition, parameter window, sampling location and criterion into the test plan before deciding how peel, sectioning, hardness and fatigue are combined; materials-side criteria align with the materials and structures and mechanical properties service scope, and joint failure localisation runs through failure analysis. The testing itself is a routine item under environmental reliability, with conditions taken from the current edition of the relevant standard and the customer technical agreement.

Scheduling is arranged per project; you can state your expected delivery date when submitting samples, and we will confirm a feasible plan against the current schedule and report progress at each milestone.

Related Q&A

Related questions

Frequently asked questions on the same topic. The first paragraph of each answer is the conclusion.

If the pull-off result passes, can the spot weld be accepted?
Not on its own - the fracture appearance is still missing. A pull-off test is a single static load: it answers whether the joint survived that load, not where it broke. Two joints can both pass with identical values and still be different parts. A button-shaped pull-out means the nugget came out intact from the base metal, so the joint is not the weak link. A flat tear along the fusion interface means the nugget never grew properly or unfused areas remain, so the margin came from nugget size rather than metallurgical bonding. Those two behave completely differently under vehicle vibration and thermal cycling. The report needs the fracture appearance and fracture location alongside the number, and usually a scaled photograph.
Can post-weld heat treatment restore a softened heat-affected zone?
It depends on the material. In steel the softened band usually comes from tempering or incomplete transformation, and post-weld heat treatment can improve structure and residual stress - but the temperature and hold time have to account for the original condition of the base metal, because on quenched and tempered steel a poorly chosen cycle will pull the base metal strength down with it. Aluminium is different: there is no phase change, and the loss in the heat-affected zone is coarsening of strengthening precipitates, which is over-ageing. Natural ageing after welding restores only the natural-ageing portion; the peak strength that was lost does not come back. Recovering it needs a full solution treatment and ageing on the whole part, which is rarely practical once components are assembled. Aluminium weld design therefore carries a joint efficiency margin rather than relying on a post-weld remedy.
A metallographic section and a peel test on the same spot weld disagree. Is that normal?
Common, and the two were never measuring the same thing. A peel test opens the joint and shows the fracture path, with the nugget edge often torn and deformed. A metallographic section grinds to a fixed plane through the centre and shows nugget size, lack of fusion, porosity and zone width on that plane. Disagreement usually has three causes: the section missed the nugget centre so the measured size reads small; the peel direction was not parallel to the nugget long axis so the failure looks worse than it is; or the two specimens came from different positions or different weld pulses. The answer is not to pick one - record where the section was taken, tie it to the peel specimen by number, and let the two pieces of evidence explain each other.

These answers share the same data source as the FAQ page.

Have a testing requirement? Send us your product details

Tell us the product model and test requirements. Our engineers will map out the test plan, the applicable standards and the item combination, and provide a quotation reference. The more specific the request, the sharper the answer.

  • Free scoping of the test plan and standards
  • Pre-scan testing during R&D to cut rework cost
  • On-site visits and witnessed testing supported
  • Scheduling per project, with progress updates at each milestone

Received — we will contact you shortly and follow up with a test plan and quotation.

By submitting you agree to be contacted by phone or email. Scheduling follows the project’s actual availability and is subject to mutual confirmation.

13510907826
Call