Key takeaways
A cracked MLCC is not one failure but two. A flex crack enters obliquely from the terminal-to-body junction, appears after assembly, and is fixed at depanelling, screw torque and connector insertion force. A thermal crack starts vertically at the solder fillet, exists right after reflow, and is fixed in the reflow profile and touch-up rules. The criterion is not whether a crack exists, but where it starts on the cross section, whether the reference designators cluster or scatter, and whether the first article after soldering already had it. Capacitance and insulation resistance can both read normal before the crack goes through, so a passed measurement is not evidence of no crack.
When an MLCC cracks, the first question is usually whether the lot is bad. What actually decides the corrective action is where the crack starts: entering obliquely from the junction between termination and ceramic body means the board was bent, while running vertically from the solder fillet at the termination means the soldering thermal excursion was too abrupt. The two sit in different places on the cross section, appear at different points in the process, and are fixed in opposite directions - one by process, one by layout and pad design.
1. Two cracks, two different origins
A ceramic capacitor is a brittle part: strong in compression, weak in tension, with almost no plastic deformation. Mounted on a board, two stress paths can break it, and they break it differently.
A flex crack starts at the junction between termination and ceramic body, on the board side. When the board bends, the solder joint holds the termination while the body follows the board, concentrating tensile stress at the junction. The crack enters the body obliquely and a single bending event often produces a diagonal crack running through both ends.
A thermal crack starts at the root of the solder fillet at the termination and runs closer to perpendicular to the board surface. It relates to the thermal gradient of the soldering process: the joint cools quickly, the termination is metal and conducts heat quickly, the ceramic body conducts slowly, the two shrink differently, and the stress releases along the interface, following the internal electrode layers.
| Criterion | Flex crack | Thermal crack |
|---|---|---|
| --- | --- | --- |
| Origin | Termination-to-body junction, board side | Root of solder fillet, along the interface |
| Direction | Oblique into the body, often through both ends | Near perpendicular to the board, may stop part way |
| Cross-section appearance | Mostly transgranular, brighter fracture | Delamination along internal electrodes, stepped |
| Distribution | Clustered at board edges, screw holes, depanelling lines, connector force direction | Weakly related to designator position, strongly related to board thickness, pad and reflow profile |
| Point in process | After assembly operations | Present right after soldering, grows with thermal cycling |
Table basis: these are general morphology criteria used in failure analysis; the actual call rests on the measured cross section and the customer technical agreement.
In one line: a flex crack is created when the board is bent during assembly, a thermal crack is created when soldering heats it too abruptly.
2. Bench tests miss it because an early crack does not change electrical parameters
This is where this failure mode slips through.
Before a crack goes through both electrode layers, the electrodes remain in parallel, the capacitance shift falls inside measurement repeatability, and nothing can be read. Insulation resistance only drops clearly after the crack has taken up moisture and a conductive path has grown. So in-circuit test passes, burn-in passes, and the failure shows up in the vehicle - not because testing was careless, but because the quantities measured are not sensitive to this defect.
A passed measurement proves the crack had not gone through at that moment. It is not evidence that no crack exists.
Two routes can force it out. The physical route is cross sectioning and polishing to see the origin, or acoustic scanning to see internal delamination; the first is conclusive but destroys the sample, the second is non-destructive but can miss very fine cracks. The stress route is to let differential expansion open the crack through temperature cycling, then let moisture in through damp heat while monitoring insulation resistance for a step drop. This is the same condition design as any environmental test, with the criterion changed from "function normal" to "did insulation fall".
One caution: if the symptom is leakage or falling insulation resistance, do not jump straight to a capacitor crack. Surface contamination and electrochemical migration take a different path; if the three conditions of ion contamination, water film and bias in electrochemical migration do not line up, come back to cracking.
3. Where mechanical stress comes from: check these five operations first
Flex cracks almost always map back to a step in the process.
| Operation | How stress arises | Where the crack lands |
|---|---|---|
| --- | --- | --- |
| Depanelling | V-cut snapping, router push, manual breaking | Designators near the depanelling line |
| Screw fixing | Uneven torque, missing washer, forced alignment across holes | A ring around the screw hole |
| Connector insertion | Insertion force lands on the joints, board is pushed into bending | Capacitors behind and beside the connector |
| Heatsink or shield pressing | Uneven pressing face, over-thick gap pad, off-centre load | Under and around the pressed area |
| Handling and test fixtures | Too few supports, pusher pins right above components | Near the fixture contact points |
The work is to map each operation onto the positional distribution of cracked designators: a column at the board edge points to depanelling, a ring around a screw hole points to torque and tightening order, a cluster behind a connector points to insertion force.
One geometric factor is often missed: the span between the two terminations. The larger the span, the greater the height difference between the ends when the board bends, and the greater the strain difference across the part. Layout therefore has to consider both distance from the stress source and the direction of the part's long axis relative to the bend. Moving a large capacitor slightly away from the edge while its long axis points straight into the bending direction usually achieves little.
4. Thermal stress: not how hot, but how fast
The input for a thermal crack is not the peak reflow temperature; it is the rate of change and the mismatch across the interface.
Thermal mass difference between termination and body. The termination is metal and heats and cools quickly; the ceramic body conducts slowly. On the same reflow profile the two experience different histories, and shear appears at the interface.
Cooling rate. Everyone watches the ramp up; the ramp down is often ignored. Cool too fast and the joint and termination carry a larger shrinkage mismatch while still relatively soft.
Touch-up soldering. An iron pressed directly on the termination raises local temperature instantly. The more touch-ups and the longer each dwell, the more thermal shock the interface sees. This is extremely common at rework stations, and rework records rarely enter the failure analysis.
Board thickness and copper area. Thick boards with large copper pours dissipate heat quickly and cool locally faster; larger parts develop a larger internal gradient.
To judge a thermal crack, pull the reflow profile and the rework records together, rather than only checking whether the oven setpoints look right.
5. How to prove which one it is
Three comparisons, and a conclusion is weak if any one is missing.
First, look at the origin on the cross section. Does the crack start obliquely at the termination-to-body junction, or vertically at the fillet root; is it transgranular, or delamination along internal electrodes. This is direct evidence, and the grinding and polishing route is the same as in terminal cross-section analysis.
Second, look at clustering in the designator map. Plot the failed designators on the board drawing: do they cluster around geometric features such as edges, holes and depanelling lines, or scatter randomly. Clustering points to mechanical stress, scattering points to incoming material or thermal. This step is non-destructive and gives a high return.
Third, align the timeline. Sample the first article after soldering for observation or scanning to establish a baseline, then sample again after assembly. Present right after soldering means thermal; appearing only after assembly means mechanical. Without that baseline, every later inference stays an inference.
One clarification: delamination and cracking on the same board are different things. PCBA delamination and popcorn is interfacial separation between laminate and copper under moisture plus fast heating - a board issue. This article is about cracking of the ceramic body itself - a component issue. The cross-section appearance and the corrective direction do not carry over, so do not merge the two in a report.
6. Outline and corrective action: what changes at each level
| Level | Action | Where to start |
|---|---|---|
| --- | --- | --- |
| Part selection | Soft termination, higher flex rating, smaller case size | Designators at board edges, screw holes and connector force direction first |
| Layout | Keep away from depanelling lines and holes, clear of pressed areas, control span and orientation | The parts aligned with the stress direction first |
| Process | Depanelling method, screw torque and tightening order, washers, touch-up rules and limits | Depanelling and screws first, then rework |
| Verification | Temperature cycling to open the crack, damp heat to admit moisture, insulation monitored during exposure | Matched one-to-one to the identified failure chain |
Of the four, part selection adds margin while process and layout reduce the input. Changing the part without changing the process consumes the margin; the problem is postponed, not removed.
For test planning, the logic of tailoring by mounting location and grouping by failure chain in the automotive environmental reliability test checklist applies directly. On the materials side, mechanical items such as bending, peel and thermal shock under materials and processes are complementary, not a substitute - they test the board and joint resistance, not cracking of the component body. At the standards level, the framework for test methods and severity classes is in GB/T 28046 and ISO 16750; specific clauses follow the customer's controlled version.
A few plain words
First, changing suppliers does not fix board bending. A certificate of conformance and "no crack after assembly" are two different things, and the former does not cover the latter.
Second, a failure report that says "capacitor cracked" without cross-section morphology, without a designator map, and without a post-solder baseline gives a conclusion, not evidence. Negotiating with a supplier on that conclusion goes nowhere.
Third, the recommended order is: look at the distribution, determine the type, change process and layout, and put part selection after that. Done the other way round, the usual outcome is two rounds of part changes with the crack still in the same place.
TMC LAB asks for the designator map, the process timeline and the rework records together before deciding which part to section - because sectioning the wrong one points the corrective action in exactly the opposite direction. If the symptom is intermittent functional anomaly rather than leakage, the diagnostic path differs; start with the reproduction sequence for intermittent failures.