Key takeaways
Weld strength is the product of three quantities: energy director geometry, material compatibility and actual melt depth. Amplitude, pressure and hold time only deliver energy; they cannot raise the ceiling set by those three. A pull-off result must be read together with the failure location. Parent-material failure means the seam is not the weak link; a clean peel around the whole interface means no real fusion; failure near the weld line means the problem is in moulding, not welding; a clip breaking first means the seam was never loaded. Glass-filled grades and mismatched grades carry a lower ceiling by nature, and moisture in nylon boils at the interface, leaving a seam that looks fine and peels in one piece. Airtightness and strength are separate criteria: a seam can leak without being weak, or be weak without leaking. Re-test after environmental exposure at the same location and in the same direction.
Weld strength on a plastic part is not something a welding machine is tuned into. It is the product of three quantities: the geometry of the energy director, whether the two materials can melt into each other at all, and how much resin truly fused at the interface. A passing pull-off force only says the seam survived that one loading; where the break happens is what tells you whether the parts are joined.
On a request form this usually reads as one line: upper and lower housings ultrasonically welded, weld strength per drawing. That line leaves out three things, namely what shape the energy director has, whether both halves are the same grade, and what moisture state the parts were in before welding. Get any one of them wrong and the same machine with the same settings will produce a good part and a cold joint.
The criteria for a weld sit at the boundary between material and structure. On one side are sampling and judgement in materials and structural testing; on the other is the sealing conclusion behind an IP rating. Both are valid, and they answer different questions.
1. Strength is three quantities multiplied, not four rows of settings
Ultrasonic welding works through friction heating at the interface. The upper part vibrates against the lower one, resin melts, flows under pressure and solidifies as one body. Amplitude, pressure, triggering method and hold time are only the means of delivering energy. What decides strength is three things at the interface.
Energy director geometry. The energy director is the small triangular ridge that melts first; its job is to concentrate energy along a controlled line. Too small a cross-section and there is not enough melt to fill the gap. Too large and more energy is needed to melt it, so the run often stops before it has travelled the full circumference.
Whether the two materials can fuse. The same resin is not the same material. Grade, glass content, flame-retardant system, mould release agent and colour masterbatch all change melting behaviour and interfacial compatibility. When the two halves come from different suppliers or different grades, the interface behaves like two liquids that do not wet each other, and pressure only presses them together.
How much actually fused at the interface. In the field this quantity is often replaced by travel distance. Travel is what the machine completed; melt depth is how deep the resin really fused and interpenetrated. Flash, gaps and part deflection sit between the two. With thin walls, poor rib placement or insufficient support, the travel completes while the melt depth never develops.
| Quantity | How it is changed on site | What goes wrong |
|---|---|---|
| --- | --- | --- |
| Energy director geometry | Change cross-section and path, add material at corners | Too small leaves insufficient melt; too large stops the run short of the full circumference |
| Material compatibility | Unify grade and colour batch, confirm glass and flame-retardant system | The interface does not fuse and strength drops to a "held together" level |
| Actual melt depth | Judge from melt depth and flash shape, not travel alone | Travel complete with shallow melt gives a cold joint that looks normal |
Of the three, the first two are fixed by the drawing and incoming material and the third by the process. That is why "the same machine fails as soon as the batch changes" is rarely a machine problem.
2. A passing pull-off force has to be read with the failure location
The pull-off test produces a number. Two parts that both pass can fail in completely different places, and the place explains completely different things.
| Failure location | What it tells you | Where to act |
|---|---|---|
| --- | --- | --- |
| Parent material breaks, seam intact | Weld is stronger than the parent; the seam is not the weak link | Stop touching weld settings; look at parent material and structure |
| Clean peel around the whole interface | No real fusion, or a contaminated interface | Check compatibility, cleanliness, melt depth and energy director |
| Cracking near the weld line or the gate | The problem is in moulding, not welding | Check gate position, weld-line temperature and mould temperature |
| Clip or rib breaks first, seam unloaded | Load never reached the seam; the test did not examine it | Change fixture and loading direction so the seam carries load |
Only one failure form proves the seam is not the weak link, and that is the parent breaking first. A part that peels around the interface may just cross the line, but its margin comes from geometry and friction fit, not from fusion.
The third row deserves its own sentence. A weld line is a weak plane formed where two flow fronts meet in the cavity; it exists in the part before any welding. Changing weld parameters will not improve a part that breaks near it.
The fourth row is a common sampling gap. The fixture grips at a clip and the loading direction lets the clip take the force first, so the seam is barely loaded. Such a pass proves the clip.
When TMC LAB takes on this kind of work, the fracture photos and the loading direction are requested before any number is discussed. A number without a fracture surface only supports the conclusion "not strong enough".
3. Glass-filled and incompatible combinations start with a lower ceiling
The difficulty with glass-filled parts is physical. Glass fibres do not melt, and molten resin has to flow between them. That flow is obstructed, so the resin available for fusion at the interface is limited from the start. The higher the glass content, the stronger the effect and the smaller the fused area that can form.
Parameters cannot compensate. They can bring a given material pair to the level that pair allows, and no further.
Another variable that gets skipped is the moisture state before welding. Nylon absorbs moisture noticeably, and a damp part heated at the interface turns that moisture into vapour, which pushes the melt apart and leaves voids and unbonded areas. It usually cannot be seen from outside, and the part peels in one piece under pull-off. The same mechanism shows up at board level, covered in moisture and popcorn delamination: vapour with nowhere to go pushes the interface open.
| Material state | Welding behaviour | What to do before submitting samples |
|---|---|---|
| --- | --- | --- |
| Same grade, dry | Even fusion, parent failure is common | Record grade, batch and drying condition |
| Same grade, damp | Voids and local unbonded areas, appearance often normal | Dry per the material datasheet and record it |
| Different grades or suppliers | No fusion, strength at a "pressed together" level | Run a compatibility trial before volume |
| Glass-filled | Small fused area, lower ceiling than the unfilled base resin | Redefine criteria for the pair, do not reuse unfilled numbers |
One drawing sent to two suppliers does not guarantee two parts of the same material. That sentence holds more strongly for welded parts than for most components.
4. Airtightness and strength are two separate criteria
A passing airtightness result and a passing weld strength result are often treated as two ways of saying one thing. They are not.
Airtightness tests connectivity: the cavity is pressurised or evacuated and the pressure or flow is watched. A seam passes as long as no through path exists, even with very shallow fusion. Strength tests load carrying: whether the interface can hold the two parts as one body.
The reverse also holds. A strong part can leak through flash, burrs or insufficient melt at a corner. The failure locations differ as well. Leaks tend to appear at corners, at the base of bosses and opposite the gate, where melt cannot reach; strength failures tend to appear where the loading direction is not parallel to the seam.
| Criterion | Question it answers | What it misses |
|---|---|---|
| --- | --- | --- |
| Pull-off force | Can the interface carry this loading | An unfused interface held by geometry |
| Airtightness or leak rate | Is there a through path | A shallow but fully closed seam |
| Sectioning and melt depth | How much fused at the interface | Uniformity around the circumference, since only the cut is visible |
| Re-test after environmental exposure | What is left after stress | Any number taken at a different point or direction |
Sectioning shows only the cut. Judging the full circumference needs multiple sections or a non-destructive method, and that has to be allowed for in the sample count, because one part answers one question.
The sealing side, including venting and cavity pressure equalisation, is covered in sealed housing pressure equalisation. That article is about vents; this one is about the seam. They do not overlap: the seam decides whether it leaks at all, the vent decides where the pressure goes.
5. The weak point of a weld often appears only after environmental exposure
A freshly welded part measures fine and drops after the environmental sequence. This feedback is common on welded parts, and the reason is simple: the seam is a step change in stiffness and material properties, so several stresses concentrate there.
Temperature cycling. The two halves differ in material and wall thickness, so they expand differently and the seam sees shear. Over enough cycles, micro defects at the interface start to grow.
Damp heat. Nylon takes up moisture and changes volume, creating internal stress at the interface; some materials also hydrolyse under damp heat and lose strength outright.
Vibration. The seam is a stiffness step and a stress concentration. When the seam is not parallel to the main vibration axis, the interface sees tearing loads.
Salt spray and chemical loads. A crevice collects liquid, and a crevice at the interface is harder to rinse and harder to dry than an open surface. How the duration for salt spray is set is covered in salt spray duration.
Applied conditions and functional status grading for these stresses sit in GB/T 28046 and ISO 16750, and the practical side of vibration is in vibration testing. The documents give conditions and criteria; they do not give a welding procedure.
For damp heat, stress cracking in plastic parts describes the other failure path: residual stress plus a medium lowers the threshold for crack initiation. Stress at the weld and moulding residual stress stack up and belong to the same chain.
Re-test at the same point and in the same direction. If the two numbers come from different points, the difference means nothing. Assembly stress also borrows part of the life in advance, as covered in assembly stress and latent damage, and welded parts are no exception: where clamping and pressing apply force is often where the crack later appears.
6. Five columns for the test plan
| Column | What to write | What goes wrong if blank |
|---|---|---|
| --- | --- | --- |
| Material and state | Both grades, glass and flame-retardant system, pre-weld drying state | After a batch change, no way to tell material drift from process drift |
| Welding method and energy director | Ultrasonic, hot plate or laser; director cross-section and path | Different results with no way to say which layer changed |
| Criteria and failure definition | Pull-off plus failure location, airtightness item, melt depth | One number only, and neither a pass nor a fail can be explained |
| Environmental sequence and re-test points | Order of cycling, damp heat, vibration and salt spray; re-test points | Two numbers from different points, so the difference is meaningless |
| Sampling and quantity | How many parts per criterion, which ones sectioned | Running short halfway and having to downgrade the conclusion |
The welding method column often gets merged into "welded per drawing". Once merged, every difference caused by a line change, a supplier change or a batch change gets filed under the vague phrase "welding quality".
A few plain words
- Weld strength is not tuned in on the machine. Settings can only bring a given material pair's interface to the level that pair allows.
- A passing pull-off force says this loading did not break it. The failure location says whether it is welded.
- A part that breaks near the weld line has a moulding problem, not a welding problem. Parameters will not help.
- Airtightness and strength are separate criteria. A seam can leak without being weak, or be weak without leaking.
- Pre-weld moisture is a column that gets skipped. Nylon boils it off at the interface, and the part looks fine until it peels in one piece.
- Re-test after environmental exposure, at the same point and in the same direction. That single rule decides whether the data is comparable.
Scheduling is arranged per project; you can state your expected delivery date when submitting samples, and we will confirm a feasible plan against the current schedule and report progress at each milestone.