Skip to main content
  1. Home
  2. Technical Blog
  3. Environmental Reliability
  4. Salt Spray Passed, the Connector Still Turned Green - Flowing Mixed Gas Tests a Different Environment, and Its Criteria Sit on Three Lines

Salt Spray Passed, the Connector Still Turned Green - Flowing Mixed Gas Tests a Different Environment, and Its Criteria Sit on Three Lines

Key takeaways

Flowing mixed gas corrosion is not a stricter salt spray. Neither replaces the other and hours do not convert. Fix the criteria first (appearance, contact resistance, insertion force), state the mated condition and the cleaning method, and make the report able to evidence the actual gas concentration.

Salt spray can pass and the connector can still turn green after a period in service. That is not a contradiction: the two tests simulate different environments. Salt spray tests chloride; flowing mixed gas tests sulphur-, nitrogen- and chlorine-bearing gases reacting inside an invisible film of water. Treating it as "a stricter salt spray" in the test plan is what gets the report questioned at audit, because the acceptance criteria do not sit on the same line at all.

1. Salt spray, mixed gas and chemical load test three different media

Start by separating the three. Salt spray atomises brine into droplets, and chloride forms soluble salts on the surface. Flowing mixed gas feeds several gases into a temperature and humidity chamber at controlled ratios, and they dissolve in a thin water film, ionise, and then react with the metal. Chemical load immerses, wipes or drops liquid reagents onto the part and tests short-term contact. The media differ, and so do the failure locations: salt spray tends to start at edges, crevices and coating damage, while gas corrosion is more uniform and starts across the whole exposed surface and through coating porosity.

TestEnvironment simulatedCriteria usually applied
---------
Salt spray (neutral / acidic / cyclic)De-icing salt, marine atmosphere, road splashCorroded area, appearance rating, loss of function
Flowing mixed gasUrban and industrial atmosphere, outgassing inside a sealed enclosureChange in contact resistance, appearance, insertion force
Chemical loadShort-term contact with fuel, cleaners, coolantAppearance, material deformation, function

There is no severity ranking among the three. A sample that passes salt spray and fails mixed gas is a common result, because the active ions differ: chloride in one case, sulphur and nitrogen in the other. Hours do not convert either; scaling salt spray hours into gas test hours has no basis in mechanism. For salt spray methods and duration levels see salt spray duration levels, and for the reagent list see GB/T 28046.5 chemical load. The whole group is scheduled under environmental reliability.

One further category is often confused with this. Electrochemical migration needs three conditions at once - an electric field, condensation, and mobile metal ions - and it shows up as falling insulation resistance or dendritic shorting, not as a discoloured connector. It is covered separately in the three paths of electrochemical migration; here it only needs to be kept apart.

2. Corrosion picks the material first, the coating structure second

Corrosion in a connector does not begin with a dirty surface; it begins with the coating structure. Two gold-plated terminals can behave differently depending on gold thickness, porosity, and whether the underlayer is nickel or copper, because those decide what the gas meets once it gets through.

SurfaceTypical reaction and appearanceWhat the report should look at
---------
SilverReacts with sulphur to form silver sulphide; bright turns dull, then blackThe rise in contact resistance, not the colour alone
CopperReacts with sulphur and chlorine; products are dark brown or greenWhether corrosion reached the base metal and penetrated the coating
TinDulls and greys; products are mostly oxides and chloridesContact resistance at crimp zones and solder joints
Gold (thin)Gold does not react; the reaction happens inside poresPorosity, gold thickness, underlayer metal

A gold layer does not stop corrosion; it relocates it into the pores. Gold is inert and the atmosphere cannot touch it, but thin gold, known in the trade as flash gold, carries pinholes. Gas enters through them and attacks the nickel or copper beneath, and the corrosion products occupy more volume than the original metal, so they extrude out of the pores and spread across the contact surface. The rise in contact resistance is not linear either: while the film is thin the reading barely moves, then it jumps at some point. That is how "it measured fine when it was fitted" and "it is intermittent a while later" can describe the same part.

Silver is more direct. In a sulphur-bearing atmosphere silver reacts almost without exception, and the silver sulphide film conducts poorly: negligible while thin, an insulator once thick. That is why silver-plated terminals inside the cabin often age worse than tin-plated ones - not because silver is poor, but because the environment contains sulphur. How the coating bonded to the substrate in the first place is covered in four entry points for coating adhesion; the state of the substrate underneath decides whether corrosion runs all the way to copper, and tests on that side are grouped under materials and processes.

3. Four stated conditions, and two quantities usually left out

Mixed gas conditions are normally written in the method standard, with the level selected by the customer standard. The method standard supplies methods and severity levels; which level applies comes from the OEM specification or the technical agreement - the same division of labour as in other environmental tests, and the laboratory does not assign the level on the customer's behalf.

ConditionWhat it decidesWho sets it
---------
Gas mixtureWhich reaction is being tested: sulphur, nitrogen and chlorine act separatelyThe methods in the standard and the OEM specification
ConcentrationReaction rate and final severity, usually expressed in parts per billionThe level of the selected method
Temperature and relative humidityThickness and continuity of the water film, which decides whether a reaction happens at allThe selected method and the OEM specification
DurationThe exposure needed to reach the criteriaOEM specification and technical agreement

Those are the stated ones. The two that get left out are different.

The first is airflow and placement. The word "flowing" in the test name is not decoration: concentration is maintained at the set value by continuous gas flow and air exchange. A sample shielding the flow upstream, sitting against the chamber wall, or a chamber loaded too full will see a lower local concentration. The same batch can produce different results at different positions. The report should record chamber position, sample orientation and load, not merely state that the standard method was followed.

The second is pre-treatment and handling. Fingers carry chloride and grease, and a contact surface that has been touched will fail earlier in a sulphur atmosphere than one that has not. The wrong cleaner leaves a film that separates the surface from the atmosphere, making the result look better than it is. Cleaning method, cleaner type and drying method must be fixed and recorded before the test. It sounds trivial, but it decides whether the report can be reproduced.

One piece of physics is worth restating: the reaction needs a water film, and humidity is the carrier. Below a certain relative humidity the reaction becomes too slow to see, which is why problems in dry regions appear late - after the warranty judgement window has closed. Temperature accelerates the reaction, but it cannot create a water film that is not there.

4. Sample state and criteria must be fixed before the chamber is opened

Sample stateWhat is actually measuredCommonly missing wording
---------
UnmatedCorrosion resistance of the whole exposed surfaceOnly "several connectors", no mated state
MatedSealing of the contact interface and contamination already present thereNo record of mating cycles before the test
Under loadWhether electrolytic or fretting effects appear with current appliedCurrent and load type not stated
No loadAtmosphere-only corrosionUnloaded by default, without saying so

Mated and unmated are not the same measurement. Once mated, the contact interface barely sees the atmosphere, and failures come mostly from two places: contamination that was already there before mating, or products extruding outward from the pores. That is why a connector can look fine in the mated state and show darkened contacts once opened. Load versus no load works the same way: whether current is applied is set by the OEM specification, but it must be stated in the report rather than assumed.

Criteria need three lines, not one.

CriterionHow it is measuredWhen it is measured
---------
AppearanceRecord discolouration and product distribution per the agreed rating methodImmediately after the test, without wiping or washing
ElectricalLow-level contact resistance, insulation resistanceAfter recovery, compared with the pre-test baseline
MechanicalInsertion force, retention forceAfter the electrical measurements

Each line answers a different question: appearance answers whether it still looks serviceable, contact resistance answers whether current still passes cleanly, insertion force answers whether it can still be mated reliably. Conflicting results are normal, so the plan must state which line triggers a failure and which is recorded only. A single criterion of "no visible corrosion" guarantees a dispute when the report is handed over.

Two sequences must not be reversed. Baseline readings have to be taken before the test; a report with post-test readings only contains numbers, not a conclusion. Corrosion products must not be wiped off before measuring: wiping destroys the appearance evidence and "repairs" the contact resistance at the same time. The correct order is to photograph and record appearance, then measure electrically, then mechanically, and leave the products for the failure analysis stage.

On the division of standards: GB/T 28046 and ISO 16750 provide environmental conditions, test methods and functional status classification, but they do not choose the corrosion level for you. Mixed gas methods and severity levels sit in the GB/T 2423.51 and IEC 60068-2-60 family, while connector measurement methods sit in the GB/T 5095 and IEC 60512 family. All condition values follow the current revision and the customer technical agreement; none are preset in this article.

A few plain words

Mixed gas corrosion is often treated as one more item to add to a list. What it actually tests is different: whether the coating structure holds up in a sulphur- and nitrogen-bearing atmosphere. The order of judgement has four steps - coating structure first (gold thickness, porosity, underlayer), then sample state (mated, loaded), then whether the conditions can be evidenced (concentration, placement, load), and only then the readings.

When TMC LAB takes on this kind of work, the mated state, the coating structure and the three criteria lines go into the test plan before the chamber is opened; the report keeps the gas concentration, the placement and the cleaning method so that a customer audit can trace them. For the wider test combination on connectors see how automotive connectors are tested; for parts on an RF path the readings are judged differently, as in the five readings on FAKRA. Conditions and criteria follow the current standard revision and the customer technical agreement.

Scheduling is arranged per project; you can state your expected delivery date when submitting samples, and we will confirm a feasible plan against the current schedule and report progress at each milestone.

Related Q&A

Related questions

Frequently asked questions on the same topic. The first paragraph of each answer is the conclusion.

Salt spray has already been done. Is mixed gas corrosion still needed?
Judge them separately, because neither replaces the other. Salt spray delivers salt droplets and tests chloride; flowing mixed gas delivers sulphur-, nitrogen- and chlorine-bearing gases that react in a thin water film, simulating urban and industrial atmospheres plus the sulphur compounds slowly released by rubber, foam and adhesives inside a sealed enclosure. Different media, different mechanisms and different criteria: salt spray is usually judged on corroded area and appearance rating, mixed gas on the change in contact resistance. Whether to include it, and at which level, follows the applicable method standard and the customer technical agreement.
Are gold-plated connectors immune to mixed gas?
Gold itself is chemically inert and does not react, but a gold layer is not a seal. Thin gold (flash gold) carries pinholes; gas enters through them and attacks the underlying nickel or copper. The corrosion products have a larger volume than the original metal, so they extrude out of the pores onto the contact surface, and contact resistance jumps at some point rather than drifting smoothly. What matters is therefore not whether gold is present, but its thickness, its porosity and the underlying structure. A porosity check before shipment is more useful than cleaning afterwards.
If the sample discolours after the test, does that mean it fails?
Not necessarily; it depends on how the criteria were written. Discoloration and electrical degradation are not the same thing. Some colour change is only a surface film while contact resistance stays in range; some parts show a clear rise in contact resistance with nothing more than slight darkening. The test plan should therefore separate three lines - appearance rating, change in contact resistance, change in insertion force - and state which one triggers a failure and which is recorded only. A single criterion such as no visible corrosion guarantees a dispute when the report is handed over.

These answers share the same data source as the FAQ page.

Have a testing requirement? Send us your product details

Tell us the product model and test requirements. Our engineers will map out the test plan, the applicable standards and the item combination, and provide a quotation reference. The more specific the request, the sharper the answer.

  • Free scoping of the test plan and standards
  • Pre-scan testing during R&D to cut rework cost
  • On-site visits and witnessed testing supported
  • Scheduling per project, with progress updates at each milestone

Received — we will contact you shortly and follow up with a test plan and quotation.

By submitting you agree to be contacted by phone or email. Scheduling follows the project’s actual availability and is subject to mutual confirmation.

13510907826
Call